DNV Grade B Steel Plate | NV B Marine Steel Plate
What is DNV Grade B / NV B marine steel plate?
DNV Grade B, officially stamped NV B on mill-approved plate, is the ordinary-strength (normal-strength) hull structural steel under DNV rules for classification – Ships that adds a 0 °C Charpy requirement where the thickness and supply-condition table calls for it. DNV implements IACS UR W11 for normal and higher strength hull steels. It shares Grade A’s minimum yield of 235 N/mm², tensile 400–520 N/mm² and 22 % minimum elongation (A5), but manganese is written as a fixed 0.80 % minimum (0.60 % if fully killed or cold-flanging) and silicon is capped at 0.35 %. In commercial enquiries it is called DNV Grade B or NV B marine steel plate.
Equivalent grades: DNV NV B ≈ ASTM A131 Grade B ≈ ABS B ≈ LR Grade B ≈ BV Grade B ≈ CCS Grade B ≈ NK KB ≈ KR RB ≈ RINA Grade B ≈ GB 712 Grade B (all class-approved, stamped by the issuing society).
Because NV B carries a 0 °C toughness guarantee where required, it is used for side shell, bottom shell and deck plating that must keep toughness near freezing, and for repair steel where the drawing allows A or B. Where the drawing calls for NV D or NV E, NV B cannot be substituted downward; supplying D or E for B is normally accepted when chemistry and tensile still meet Grade B.
Plates that pass mill tests under DNV survey are die-stamped or stencilled NV B (plus Z or U where through-thickness or ultrasonic requirements apply) and are supplied with a mill certificate the DNV Surveyor endorses. SHH STEEL supplies NV B plate from Chinese mills that hold DNV works approval for the grade, from stock in common sizes or from a mill rolling cycle, with DNV survey arranged at the mill.
DNV NV B plate: specification summary
| Item | DNV NV B / Grade B data |
|---|---|
| Rule basis | DNV rules for classification – Ships (metallic materials / rolled steel for hull); IACS UR W11 normal-strength Grade B |
| Strength level | normal (ordinary) strength, yield strength ReH 235 N/mm² min. |
| Plate thickness primarily covered | up to 100 mm under IACS UR W11 scope for plates; greater thickness by special consideration (see UNCERTAIN) |
| Steelmaking | basic oxygen, electric furnace or open-hearth, or other process specially approved by DNV |
| Deoxidation | killed or semi-killed ≤50 mm; killed >50 mm |
| Fine grain | not mandatory for all thicknesses (see UR W11 Table 1 / supply table) |
| Condition of supply | per UR W11 Table for Grade B (AR/CR/N/TM by thickness — confirm on PO) |
| Impact test | Charpy at 0 °C where the thickness/condition table requires (often none ≤25 mm; required in heavier bands) |
| Marking | NV B (commercial “DNV Grade B”); plus Z / U / TM where ordered and qualified |
| Thickness tolerance | IACS UR W13 as adopted by DNV (minus tolerance commonly 0.3 mm class — confirm on PO; see UNCERTAIN) |
| Certificate | mill certificate endorsed by the DNV Surveyor; EN 10204 3.1 / 3.2 on request |
Size range. NV B is rolled on wide plate mills in China from about 5 mm to 100 mm and more, widths 1500–3500 mm and lengths up to about 18 m depending on mill; 6–25 mm plate in 1800–2500 mm width is the bulk of the market. Plates under about 6 mm are often cut from DNV-approved hot-rolled coil, which needs separate approval of the coil process. Ask for confirmation for plates over 100 mm or wider than 3200 mm.
DNV Grade B / NV B chemical composition (heat and product analysis)
| Element | Heat (ladle) analysis, % | Product (check) analysis, % | Note |
|---|---|---|---|
| C | 0.21 max. | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | plates; sections may differ where notes allow |
| Mn | 0.80 min. (0.60 min. if fully killed or cold-flanging) | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | Note allows 0.60 % min. when fully killed or cold-flanging |
| Si | 0.35 max. | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | |
| P | 0.035 max. | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | |
| S | 0.035 max. | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | lower S may be agreed for cold-flanging quality |
| Cu | to be determined and reported | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | residual / intentionally added — report when present (IACS UR W11 Table 1 notes) |
| Cr | to be determined and reported | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | residual / intentionally added — report when present (IACS UR W11 Table 1 notes) |
| Ni | to be determined and reported | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | residual / intentionally added — report when present (IACS UR W11 Table 1 notes) |
| Mo | to be determined and reported | numeric tolerance not tabulated in DNV rules – agree on order / mill certificate | residual / intentionally added — report when present (IACS UR W11 Table 1 notes) |
| C + Mn/6 | 0.40 max. | not applicable (calculated from heat analysis) | carbon + 1/6 manganese cap |
Product (check) analysis column: DNV rules specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.
Source: IACS UR W11 Table 1 (ladle samples) for normal-strength Grade B — the chemistry DNV applies to NV B hull plate. Heat (ladle) analysis is determined by the mill on each heat and must meet Table 1. Product (check) analysis on the finished plate is not given numeric tolerances in UR W11 itself; W11 4.2 accepts the manufacturer’s declared analysis subject to occasional Surveyor checks. When a purchaser or Surveyor requires product analysis on the certificate, ask at enquiry and record the agreed tolerances — do not invent numbers.
Grade B is the only ordinary-strength grade with a fixed 0.80 % Mn minimum (reducible to 0.60 % when fully killed or ordered cold-flanging). Silicon is capped at 0.35 %, tighter than Grade A’s 0.50 %. In practice Chinese mills supply aluminium-killed NV B; treat typical ladle figures as indicative only and check the actual mill certificate.
DNV NV B tensile properties
| Property | Requirement (IACS UR W11 Table 6) |
|---|---|
| Tensile strength Rm | 400–520 N/mm² |
| Yield strength ReH | 235 N/mm² min. (or Rp0.2 where ReH cannot be determined) |
| Elongation A5 | 22 % min. (5.65 √S0) |
| Impact test temperature | 0 °C |
On the 200 mm gauge full-thickness flat specimen (25 mm width), minimum elongation depends on thickness:
| Thickness (mm) | ≤5 | >5–10 | >10–15 | >15–20 | >20–25 | >25–30 | >30–40 | >40–50 |
|---|---|---|---|---|---|---|---|---|
| Elongation min. % | 14 | 16 | 17 | 18 | 19 | 20 | 21 | 22 |
All four normal-strength grades share these tensile values. For each batch, one tensile test is taken from one piece (extra tests when finished weight exceeds 50 t, and for every 10 mm variation in thickness from the same cast), unless otherwise agreed by DNV.
DNV NV B: Charpy at 0 °C and supply condition
CVN at 0 °C where thickness/condition table requires (typically >25 mm). Deoxidation: killed or semi-killed ≤50 mm; killed >50 mm. Average energies at 0 °C (full-size specimens, long / trans) per IACS UR W11 Table 6:
| Thickness | Longitudinal (J min.) | Transverse (J min.) |
|---|---|---|
| t ≤ 50 | 27 | 20 |
| 50 < t ≤ 70 | 34 | 24 |
| 70 < t ≤ 100 | 41 | 27 |
One individual value may fall below the average if it is at least 70 % of it. Generally only longitudinal specimens are prepared unless the purchaser or DNV asks for transverse. The test frequency and permitted delivery condition (AR, CR, N or TM) follow the UR W11 supply-condition table for Grade B, so write the condition into the PO. Beyond 100 mm thickness is special consideration with DNV (see UNCERTAIN).
Thickness tolerance and surface condition
DNV applies the thickness tolerances of IACS UR W13 (Thickness tolerances of steel plates and wide flats) unless the purchase order states otherwise. In practice class-approved hull plate is ordered to the class minus-tolerance band commonly associated with UR W13 (often 0.3 mm minus — confirm the exact class and plus tolerance on the PO; see UNCERTAIN). Plus tolerance, flatness, width and length follow the agreed national or international standard (for example ASTM A6 or EN 10029) unless specified otherwise.
Surface quality follows a recognised standard such as EN 10163 parts 1–2 (or equivalent accepted by DNV). Surface defects may be ground within UR W11 limits; grinding areas are checked so remaining thickness stays within the allowed minus tolerance. If you plan to shot-blast and prime at the yard, state any surface class on receipt in the order.
DNV NV B plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Condition | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1800 / 2000 | 6000 / 8000 | AR / CR | 100+ t | China |
| 8 | 1800 / 2000 | 8000 / 12000 | AR / CR | 200+ t | China |
| 10 | 2000 / 2200 | 8000 / 12000 | AR / CR | 200+ t | China |
| 12 | 2000 / 2200 / 2500 | 12000 | AR / CR | 200+ t | China |
| 14 | 2000 / 2200 | 12000 | AR / CR | 100+ t | China |
| 16 | 2000 / 2500 | 12000 | AR / CR | 200+ t | China |
| 20 | 2000 / 2500 | 12000 | AR / CR | 100+ t | China |
| 25 | 2200 / 2500 | 12000 | AR / CR | 100+ t | China |
| 30 | 2200 | 10000 / 12000 | AR / CR | 100+ t | China |
| 40 | 2200 | 10000 | AR / CR | 50+ t | China |
| 50 | 2200 | 8000 / 10000 | AR / CR | 50+ t | China |
Quantities are approximate and change daily (indicative — confirm before booking); all stock plates carry NV B marking and DNV-endorsed mill certificates when sold as DNV class plate. Sizes outside the table (for example 3000 mm width, 60–100 mm thickness, or fixed lengths for a cutting plan) are produced in the next mill rolling cycle, typically 3–6 weeks including DNV survey. Send your size list and we will reply with what is in stock and what must be rolled.
Packing. Plates are bundled by size with steel strapping, marked with heat number, grade and DNV stamp, and shipped in containers (up to about 11.8 m) or break bulk for longer plates.
DNV NV B equivalents in other rules and standards
| Standard / society | Designation | Comment |
|---|---|---|
| DNV | NV B (DNV Grade B) | this page; stamped under DNV survey |
| ASTM A131/A131M | ASTM A131/A131M Grade B | same base chemistry and tensile band; A131 is a product standard, not class approval |
| ABS | ABS B | IACS UR W11 ordinary-strength; stamped AB/B |
| LR | LR Grade B | IACS UR W11 |
| BV | BV Grade B | IACS UR W11 |
| CCS | CCS B | IACS UR W11 |
| NK (ClassNK) | NK KB | ClassNK designation KB |
| KR | KR RB | KR designation RB |
| RINA | RINA Grade B | IACS UR W11 |
| GB 712 | GB 712 Grade B | Chinese ship steel standard; GB 712 alone is not class approval |
| ASTM A36 | ASTM A36 | similar strength band but not a hull steel; no class marking |
| EN 10025-2 | EN 10025-2 S235JR / S235J0 / S235J2 | structural; J0 has 0 °C test, J2 −20 °C |
| JIS G3106 | JIS G3106 SM400A / SM400B | welded-structure steel; SM400B adds a 0 °C test |
These are comparisons, not substitutions. A DNV-classed hull needs plate made by a mill approved by DNV for this grade and certified under DNV survey. Dual or multi-class certification (for example DNV + ABS, or DNV + CCS) can be arranged at the mill when the heat is surveyed by both societies.
DNV NV B vs NV A/B/D/E and vs structural steels
All four normal-strength grades share the same 235 N/mm² yield and 400–520 N/mm² tensile range; they differ in deoxidation and toughness. Compared with NV A, Grade B adds the 0 °C impact requirement in the thicknesses the supply table covers; Grade A still needs no CVN up to 50 mm. Grade D (−20 °C) and Grade E (−40 °C) go further for colder service. The hull steel grade for each strake is set by the classification rules according to structural member category and thickness, so check the approved drawing first. Sheer strakes, bilge strakes, deck stringers and ice-belt plating usually call for B, D, E or higher-strength plates under DNV GL Steel Plates.
Compared with land structural steels, NV B is close in strength to ASTM A36, ASTM A283 Grade C and S275JR class steels but differs in class thickness tolerance practice, the C + Mn/6 ≤ 0.40 cap, and above all the DNV survey and NV B stamp. For a DNV-classed vessel only DNV-certified plate is accepted.
When DNV NV B is the right choice: typical uses are hull plating and members that the material class assigns a 0 °C toughness level, typically in the thicker range where Grade A is no longer accepted — side shell, bottom shell and deck plating near freezing, and repair steel where the drawing allows A or B. The Charpy temperature (0 °C) is fixed by the letter B, and the strength by the normal-strength level (ReH 235 N/mm²). Pick the strength from the scantling calculation and the letter from the material class and design temperature on the approved drawing. Swapping to a different letter or strength needs class approval of the drawing change, not just a new purchase order.
Applications, cutting and welding of DNV NV B
Typical uses: side and bottom shell in temperate-to-cool service, strength deck plating where 0 °C is specified, inland and coastal vessels with thicker Grade B members, pontoons and barges that outgrow Grade A, and ship-repair replacement steel. Offshore and port structures also use ordinary-strength grades for secondary steel; see offshore platform steel plates for primary structure grades.
Cutting: oxy-fuel, plasma and laser cutting all work without preheat in normal thicknesses. Welding: with C + Mn/6 at or below 0.40 %, NV B is welded with ordinary-strength consumables approved for the grade and 0 °C toughness level required by the shipyard’s DNV-approved WPS; preheat is generally unnecessary below about 25–30 mm except in cold or humid conditions — follow your approved welding procedure, not a generic number from a catalogue. Forming: plates intended for cold flanging should be ordered with the flanging quality agreed on the PO.
Processing notes for NV B: cold forming and flanging of normal-strength plate are routine. Keep the cut edges of plate thicker than 50 mm free of notches, because thick plate of this grade is controlled more tightly for deoxidation (killed or semi-killed ≤50 mm; killed >50 mm).
Certificates, DNV survey and third-party inspection
Every plate is tested and marked at the mill under DNV survey; the mill certificate lists heat number, ladle chemistry (elements required by UR W11 Table 1, plus intentionally added elements), tensile results, impact results at 0 °C where required, condition of supply and plate numbers, and is endorsed by the attending Surveyor. On request we add EN 10204 3.2 certificates with third-party witness by TÜV, SGS, BV or another agency, ultrasonic testing (U mark) or through-thickness testing (Z mark), and multi-class certification with other major class societies (ABS, LR, BV, CCS, NK, KR, RINA).
On receipt, check: NV B stamp and heat number on each plate match the certificate; the certificate shows DNV endorsement, not just a mill stamp; thickness at several points meets the ordered UR W13 / PO tolerance; impact results agree with the table below for the delivered thickness.
Charpy acceptance for NV B by thickness (from IACS UR W11 Table 6; actual results as per standard and mill certificate):
| Thickness t (mm) | Test temperature | Average energy, longitudinal (J min.) | Average energy, transverse (J min.) |
|---|---|---|---|
| t ≤ 50 | 0 °C | 27 | 20 |
| 50 < t ≤ 70 | 0 °C | 34 | 24 |
| 70 < t ≤ 100 | 0 °C | 41 | 27 |
On receipt, check that the test temperature is 0 °C and that the energy matches the band for the delivered thickness. Also check that the plate number on the stamp matches the certificate line, and that the DNV Surveyor endorsement is present. If UT was ordered (e.g. EN 10160 or ASTM A578 level), check the UT report as well. If the PO asked for 3.2, the inspector’s report must name the witnessed tests and plate numbers.
Common mistakes when ordering DNV Grade B / NV B
- Ordering “DNV B” without requiring DNV certification (NV B stamp + Surveyor-endorsed certificate)
- Accepting Grade A certificates for a Grade B PO (missing 0 °C impact where required)
- Ignoring Mn 0.80 % min. (or 0.60 % when fully killed / cold-flanging) on the ladle analysis
- Substituting NV B where the drawing requires NV D or NV E
- Coil-cut plate without DNV coil-process approval
- Confusing Grade B with higher-strength NV A32 / AH32
Each of these is avoided by writing the requirement into the purchase order and checking it on the certificate before the plates are cut.
Sourcing DNV NV B plate: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Fake or re-stamped class plate | plates from DNV-approved mills only; certificate and NV B stamp traceable to the heat; third-party witness and EN 10204 3.2 on request |
| Unsafe deposit or payment risk | T/T or L/C payment; inspection before balance payment |
| Small quantities across many sizes | mixed thicknesses and grades (NV B, NV A, NV A36, etc.) combined in one container or shipment |
| Slow delivery | dedicated staff follow each order with weekly production and shipping updates and photos |
| Cutting and preparation | own workshop for cutting to size, bevelling, drilling and machining before shipment |
How to order DNV NV B plate
State the grade and rule (DNV NV B / DNV Grade B, DNV rules for ships – metallic materials), whether multi-class certification is needed, thickness, width, length and quantity per size, condition of supply, any Z or U requirement, surface or primer requirements, certificate type (mill certificate with DNV endorsement, EN 10204 3.2 with third-party witness), packing and destination port. Send the list to SHH STEEL for price, available stock and lead time.
Sample PO line: “Steel plate to DNV rules for classification – Ships, Grade B (NV B), delivery condition [AR/CR/N/TM], 20 × 2500 × 12000 mm, 30 pcs, marked NV B, certificate endorsed by DNV Surveyor, EN 10204 3.2 [if required], UT [if required], CIF [port].” Each bracketed item changes price, lead time and which mills can supply, so fix them at enquiry stage.
FAQ
Conclusion
DNV Grade B / NV B is ordinary-strength hull steel under DNV rules and IACS UR W11: 235 N/mm² minimum yield, 400–520 N/mm² tensile, Charpy at 0 °C where required, and class survey with the NV B stamp. What the rules leave open has to be fixed in the order: DNV (or multi-class) certification, the supply condition and impact testing, whether product analysis is required on the certificate, the thickness-tolerance class, and the certificate type (3.1 vs 3.2).
SHH STEEL supplies NV B plate rolled by Chinese mills that hold DNV works approval for the grade, so every plate carries the NV B stamp and a Surveyor-endorsed certificate traceable to its heat. Common thicknesses are available from stock; other sizes are scheduled into the mill rolling cycle with DNV survey arranged at the mill. On request we add EN 10204 3.2 certificates with third-party witness (TÜV, SGS, BV or another agency) and joint certification with ABS, LR, BV, CCS, NK, KR or RINA.
We accept T/T or L/C payment, with inspection before the balance is paid. Small quantities in several sizes, or NV B mixed with NV A, NV D or higher-strength grades such as NV A36, can be combined in one container. A dedicated coordinator sends production and shipping updates with photos, and our own workshop cuts to size, bevels, drills and machines plates before shipment so they arrive ready for fabrication.
Request a quotation: send SHH STEEL the grade (NV B / DNV Grade B), thickness, width, length, quantity per size and destination port, plus any multi-class, Z/U or 3.2 certificate requirement. We reply with price, available stock and lead time.