ASTM A264 SA516 Gr.70 + 304L Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 304L stainless steel clad plate bonds a low-carbon 304L layer to a pressure vessel carbon steel base by explosion or roll bonding. It suits nitric acid, food and water service where molybdenum is not needed. SHH STEEL produces it in common thickness pairs, tested for 140 MPa bond shear and ultrasonic integrity.
Keywords
304L stainless steel clad plate, ASTM A264 304L clad plate, SA516 Gr.70 + 304L, ASME SA 264, 304L clad steel plate
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 304L = S30403 / 1.4307
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 304L stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 304L stainless steel clad plate is a bimetal pressure vessel plate made of a 304L (UNS S30403) low-carbon austenitic stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 304L face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

Fabricators usually write it as SA516 Gr.70 + 304L followed by the thickness pair, for example 3 + 16 mm, cladding first. 304L is the plain 18-8 austenitic grade with carbon held to 0.030 % maximum, so it is the most economical stainless cladding for duties that do not involve chlorides. In a 19 mm shell, a 3 mm 304L layer replaces what would otherwise be 19 mm of solid stainless steel, and the carbon steel does the structural work at a fraction of the alloy cost.

Buyers tend to choose 304L clad plate for one of three reasons: the medium is oxidizing, such as nitric acid, where molybdenum adds nothing; the product must stay clean, as in food, beverage and water service; or the vessel will see welding and stress relief that would sensitize a higher-carbon 304.

SHH STEEL can produce 304L clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 304L clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 304L
Cladding A240 / SA-240 304L, UNS S30403
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A complete order line for this plate reads: “Clad plate to ASME SA-264, cladding SA-240 304L, 3 mm minimum; base SA-516 Grade 70, 16 mm minimum; Class 1 bond quality, 100 % UT (S12); shear test required; finish pickled.” For nitric acid equipment it is worth adding the corrosion test the plant specification asks for, because A264 lists corrosion testing as an item for the purchaser to state, not as a default.

SA516 Gr.70 base and 304L cladding

The two layers of SA516 Gr.70 + 304L are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 304L for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 304L is specified as the cladding

304L (ASME SA240 304L) contains 18.0 to 20.0 % chromium and 8.0 to 12.0 % nickel with no molybdenum. Its low carbon limits chromium carbide formation at grain boundaries during the heat cycles a clad plate goes through: bonding, flattening, stress relief and the vessel’s own post-weld heat treatment. That makes it a safer choice than standard 304 whenever the SA516 base has to be stress relieved.

Its weak point is chloride. In warm, chloride-bearing water 304L can pit and suffer stress corrosion cracking, which is why engineers move to 316L, duplex 2205 or higher alloys for brackish water, chloride process streams and coastal splash zones. In nitric acid the picture reverses: 304L is often preferred to 316L, because molybdenum gives no benefit in strongly oxidizing acid.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

304L compared with other austenitic claddings

Cladding C max, % Mo, % Choose it when
304L (S30403) 0.030 — Oxidizing acids, food and water service, welded and stress relieved vessels
304 (S30400) 0.08 — No PWHT and a higher minimum yield is useful
316L (S31603) 0.030 2.00 – 3.00 Chlorides or reducing acids where 304L pits
321 (S32100) 0.08 — Intermittent service in the sensitizing range, 425 to 815 °C

Explosion bonded and roll bonded 304L clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 304L plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

For 304L the two routes give the same cladding chemistry, because neither process melts the alloy. Thin 2 mm claddings on large tank plates are often roll bonded; thick clad tube sheets for nitric acid coolers are explosion bonded.

Chemical composition of 304L cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 304L clad plate is certified layer by layer: the 304L cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

304L cladding (UNS S30403)

Element 304L cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.030 max 0.005 over max ≤ 0.035
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.045 max 0.010 over max ≤ 0.055
Sulfur (S) 0.030 max 0.005 over max ≤ 0.035
Silicon (Si) 0.75 max 0.05 over max ≤ 0.80
Chromium (Cr) 18.0 – 20.0 0.20 under min / 0.20 over max 17.80 – 20.20
Nickel (Ni) 8.0 – 12.0 0.15 under min / 0.15 over max 7.85 – 12.15
Nitrogen (N) 0.10 max 0.01 over max ≤ 0.11
Iron (Fe) Balance — —

The limits are those of A240 for UNS S30403. The product analysis column is the heat limit widened by the A480 tolerance, which is set by the maximum of the specified range and applies below the minimum and above the maximum. The carbon line is the one to watch: a 304L cladding that drifts above 0.035 % on product analysis loses the reason it was specified.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 304L clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 304L cladding (A240) SA516 Gr.70 base
Tensile strength 485 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 170 MPa min 260 MPa min
Elongation 40 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 201 HBW / 92 HRBW max Not specified

SA516 Gr.70 sits on the first row of the tensile table, so a 3 + 16 mm SA516 Gr.70 + 304L plate is tested full thickness and the composite must fall between 485 and 655 MPa. The softer 304L layer pulls the composite down only slightly; problems are rare. A 5 + 40 mm plate exceeds 38 mm and is tested on base steel only.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Clad tube sheets for nitric acid coolers are normally ordered Class 1 with 100 % coverage.

Heat treatment of SA516 Gr.70 + 304L clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

Many explosion bonded 304L plates are delivered as-clad and flattened, or stress relieved by agreement, because a full solution treatment at stainless steel temperatures would also take the SA516 base through a cycle it was not designed for. Roll bonded plates come out of the mill’s normal heat treatment. Either way, the low carbon of 304L is what lets the cladding go through the base steel’s stress relief without serious sensitization.

For nitric acid service, purchasers often add an intergranular corrosion test of the cladding after the final heat treatment, such as an ASTM A262 practice agreed at the order. Specify the practice and acceptance level in the purchase order, together with any simulated PWHT the coupons must see first.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

We recommend ordering 304L cladding as a minimum thickness, typically 2 or 3 mm, so the design corrosion allowance survives any grinding of surface marks. The 304L face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 304L clad plate

SA516 Gr.70 + 304L clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 304L; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 8 10 Food and water tanks
2 + 10 12 Atmospheric storage tanks
3 + 10 13 Low-pressure vessels, ducts
3 + 12 15 Vessel shells and dished heads
3 + 14 17 Nitric acid tanks
3 + 16 19 Columns and absorbers
3 + 20 23 Reactors, exchanger shells
3 + 25 28 Heavier shells
4 + 30 34 Heads with higher corrosion allowance
5 + 40 45 Small tube sheets
6 + 50 56 Clad tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 304L clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 304L surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309L type filler, which tolerates dilution from the carbon steel and still leaves an austenitic deposit.
  5. Cap with 308L filler so the surface layer matches 304L, then pickle and passivate the weld zone.

For 304L, the 309L buffer and 308L cap are the standard pairing. Keep the interpass temperature moderate, as for any austenitic overlay. Where only steel-side access is available, the stainless part of the joint is welded with stainless fillers from the cladding upward and the carbon steel completed afterwards.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 304L stainless steel clad plate

304L stainless steel clad plate is used where a carbon steel pressure shell needs a clean, corrosion-resistant inner face and the medium does not call for molybdenum.

  • Nitric acid plants: absorption columns, bleachers, storage tanks and coolers.
  • Fertilizer units handling ammonium nitrate solutions.
  • Food, dairy and beverage tanks and process vessels.
  • Water treatment vessels for demineralised and low-chloride water.
  • Pharmaceutical and fine chemical vessels for non-chloride media.
  • Heat exchanger shells and channels on clean steam and condensate.

When 304L is the wrong choice

If the process water carries chlorides above a few hundred mg/L at elevated temperature, or the vessel sits in a marine atmosphere, 304L is likely to pit. Move to 316L, 2205 or a higher alloy; a clad plate makes that upgrade cheap because only the cladding changes.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 304L Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Intergranular corrosion test of cladding ASTM A262 practice, by agreement Nitric acid service; when ordered
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 304L, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 304L UNS S30403 1.4307 (X2CrNi18-9) SUS304L 022Cr19Ni10 (S30403)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

For Japanese projects the same plate is ordered to JIS G3601 with SUS304L cladding; Chinese projects use GB/T 8165 or NB/T 47002.1 with S30403 on Q345R. The EN and GB grades are close, not identical, substitutes, so check them against the design code.

Why order 304L clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 304L orders we often handle nitric acid equipment, where buyers value a cladding carbon check on the certificate and a clear statement of the final heat treatment.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

Is 304L or 316L better for clad plate?
It depends on the medium. 304L is the economical choice for nitric acid, food and water service. 316L, with 2 to 3 % molybdenum, is better where chlorides cause pitting. Both have 0.030 % maximum carbon and the same welding approach.
Can 304L clad plate be used in nitric acid?
Yes; it is one of its main uses. The low carbon limits sensitization during bonding and stress relief. Many plant specifications add an intergranular corrosion test of the cladding, which must be stated on the order.
Which filler metals are used for SA516 Gr.70 + 304L?
Carbon steel filler for the base, a 309L buffer over the carbon steel weld on the clad side, and a 308L cap. Carbon steel filler must not touch the cladding.
What thickness of 304L cladding should I order?
Usually 2 to 3 mm minimum, set by the corrosion allowance plus a margin for grinding. Tube sheets often use 5 to 8 mm so that tube holes and seal welds sit wholly in the cladding.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 304L cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 304L Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 304L stainless steel clad plate pairs an A240 304L layer with an SA516 Grade 70 base, bonded by explosion or roll bonding, with 140 MPa minimum shear strength when specified and ultrasonic bond quality Class 1, 3 or 5. It is the economical clad choice for nitric acid, food and water duties.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *