ASTM A264 SA516 Gr.70 + 2205 Duplex Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 2205 duplex stainless steel clad plate bonds S32205 duplex cladding to a carbon steel pressure vessel base. It resists chloride pitting and stress corrosion cracking far better than 316L. SHH STEEL produces it by explosion bonding and roll bonding, with 140 MPa bond shear and ultrasonic tests when ordered.
Keywords
2205 duplex stainless steel clad plate, duplex clad plate, ASTM A264 2205, SA516 Gr.70 + 2205, S32205 clad plate
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 2205 = S32205 / 1.4462
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 2205 duplex stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 2205 duplex stainless steel clad plate is a bimetal pressure vessel plate made of a 2205 (UNS S32205) duplex stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 2205 face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

The usual notation is SA516 Gr.70 + 2205 or SA516 Gr.70 + S32205 with the thickness pair, for example 3 + 20 mm. 2205 is a duplex stainless steel with a roughly balanced structure of austenite and ferrite, 22 % chromium, 3 % molybdenum and added nitrogen. As a cladding it gives a duplex clad plate with much better resistance to chloride stress corrosion cracking than any 300-series grade, at a fraction of the cost of solid duplex plate.

Duplex clad plate is a newer choice than 316L clad, and it brings some extra points to settle at the order: heat treatment, ferrite content and how the vessel’s PWHT will affect the duplex structure. The sections below cover each one.

SHH STEEL can produce 2205 clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 2205 clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 2205
Cladding A240 / SA-240 2205, UNS S32205
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

An order line reads: “Clad plate to ASME SA-264, cladding SA-240 UNS S32205, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1 bond quality, 100 % UT; shear test required; heat treatment as agreed; ferrite content and intermetallic phase testing as agreed.” A264 deliberately leaves duplex heat treatment to agreement, so the order must fill that gap.

SA516 Gr.70 base and 2205 cladding

The two layers of SA516 Gr.70 + 2205 are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 2205 for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 2205 is specified as the cladding

2205 (ASME SA240 2205) contains 22.0 to 23.0 % chromium, 4.5 to 6.5 % nickel, 3.0 to 3.5 % molybdenum and 0.14 to 0.20 % nitrogen. Using the minimum values, its pitting resistance equivalent (Cr + 3.3 Mo + 16 N) is about 34, against about 23 for 316L. In practice that means a much higher margin against pitting and crevice corrosion in chloride water.

The ferrite phase is what gives 2205 its resistance to chloride stress corrosion cracking, the failure mode that limits 304L and 316L in hot chloride service. Duplex also has more than double the yield strength of 316L, 450 against 170 MPa, which helps resist erosion and mechanical damage on the clad face.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

2205 compared with 316L and 904L cladding

Cladding PREN (min. analysis) Yield min, MPa Chloride SCC resistance
316L (S31603) about 23 170 Limited in hot chlorides
2205 (S32205) about 34 450 Good
904L (N08904) about 32 220 Better than 316L; best in sulfuric acid
2507 (S32750) about 38 550 Very good; seawater duty

Explosion bonded and roll bonded 2205 clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 2205 plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

Explosion bonding is the main route for 2205 clad plate: it bonds the duplex layer without melting, and the ferrite-austenite balance of the cladding is set by its own prior heat treatment. In roll bonding, the pack’s rolling and heat treatment cycle must suit both the duplex cladding and the carbon steel.

Chemical composition of 2205 cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 2205 clad plate is certified layer by layer: the 2205 cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

2205 cladding (UNS S32205)

Element 2205 cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.030 max 0.005 over max ≤ 0.035
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.030 max 0.005 over max ≤ 0.035
Sulfur (S) 0.020 max 0.005 over max ≤ 0.025
Silicon (Si) 1.00 max 0.05 over max ≤ 1.05
Chromium (Cr) 22.0 – 23.0 0.25 under min / 0.25 over max 21.75 – 23.25
Nickel (Ni) 4.5 – 6.5 0.10 under min / 0.10 over max 4.40 – 6.60
Molybdenum (Mo) 3.0 – 3.5 0.10 under min / 0.10 over max 2.90 – 3.60
Nitrogen (N) 0.14 – 0.20 0.02 under min / 0.02 over max 0.12 – 0.22
Iron (Fe) Balance — —

These are the A240 limits for UNS S32205, the tighter version of the older S31803. Nitrogen is the element to check on the certificate: it stabilizes austenite, adds strength and pitting resistance, and is what gives the weld zone a chance to keep a balanced structure.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 2205 clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 2205 cladding (A240) SA516 Gr.70 base
Tensile strength 655 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 450 MPa min 260 MPa min
Elongation 25 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 293 HBW / 31 HRC max Not specified

Duplex cladding brings a particular tensile issue. A 3 + 20 mm plate is tested full thickness, and the composite must not exceed the base maximum plus 35 MPa, that is 655 MPa. Because the 2205 layer is much stronger than SA516 Gr.70, a thick cladding on a strong base can push the composite toward that ceiling. If the cladding is ordered as corrosion allowance only, A264 lets the tensile test exclude it, which removes the problem; state this on the order when it applies.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Duplex clad tube sheets and heads are normally ordered Class 1 with 100 % coverage.

Heat treatment of SA516 Gr.70 + 2205 clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

For duplex cladding, A264 says only that the heat treatment is agreed between purchaser and manufacturer. Explosion bonded 2205 plate is commonly supplied as-clad and flattened, using cladding that was solution annealed before bonding. A full solution anneal after bonding would restore the duplex structure but would also take the carbon steel far above its normal range, so it is rarely chosen.

The bigger question is the vessel’s PWHT. Holding duplex steel in the intermetallic range can form sigma phase, which reduces toughness and corrosion resistance. Many projects therefore qualify the PWHT on S3 coupons and add a test for detrimental intermetallic phases, for example to ASTM A923, together with a ferrite measurement. GB/T 8165 sets 40 to 60 % ferrite for duplex cladding; under A264 the range is agreed.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 2205 layer to a minimum thickness, typically 2 to 3 mm; its strength and erosion resistance often allow a thinner cladding than 316L for the same service. The 2205 face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 2205 clad plate

SA516 Gr.70 + 2205 clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 2205; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 10 12 Scrubber and absorber shells
2 + 12 14 Desalination evaporator shells
3 + 12 15 Vessel shells and heads
3 + 16 19 FGD absorbers
3 + 20 23 Pressure vessels, separators
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Tube sheets
6 + 50 56 Clad tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 2205 clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 2205 surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309LMo type filler, or another buffer qualified for duplex overlay on carbon steel.
  5. Cap with 2209 duplex filler, which is over-alloyed in nickel to give a balanced weld structure, then pickle and passivate the weld zone.

Duplex welding is about balance. Too little heat input leaves too much ferrite; too much heat input or high interpass temperature risks intermetallic phases. Qualify the procedure with ferrite measurements and, where the project requires, corrosion or impact testing of the weld overlay.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 2205 duplex clad plate

2205 duplex clad plate is used where chloride levels or temperatures are too high for 316L, but solid duplex would be heavier or more expensive than needed.

  • Desalination: evaporator shells and water boxes in thermal plants.
  • Flue gas desulfurization absorbers and ducts with chloride-bearing slurry.
  • Oil and gas separators and produced water vessels.
  • Pulp and paper digesters and bleach plant towers.
  • Chemical vessels handling chloride-bearing process streams.
  • Heat exchanger shells and tube sheets on brackish water.

When to go beyond 2205

For seawater at elevated temperature or strong acid chlorides, super duplex 2507 or nickel alloys such as 625 and C276 become the candidates. Our nickel alloy clad plates section covers those.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 2205 Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Ferrite content and intermetallic phase test Agreed method, e.g. ASTM A923 When ordered; common for duplex
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 2205, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 2205 UNS S32205 1.4462 (X2CrNiMoN22-5-3) SUS329J3L 022Cr23Ni5Mo3N (S22053)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Chinese projects order the same product as S22053 + Q345R under GB/T 8165 or NB/T 47002.1; GB/T 8165 makes outer bend tests and ferrite checks mandatory for duplex cladding. Japanese projects use SUS329J3L under JIS G3601.

Why order 2205 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 2205 orders we agree heat treatment, ferrite range and PWHT simulation in writing before production.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

Is 2205 duplex clad plate better than 316L clad plate?
For chloride service, yes. 2205 has a PREN of about 34 against 23 for 316L, resists chloride stress corrosion cracking, and has 450 MPa minimum yield. In mild media 316L is cheaper and easier to weld.
What ferrite content should 2205 cladding have?
A264 does not set one. GB/T 8165 requires 40 to 60 % for duplex cladding, and many project specifications use a similar range. State the range and method on the order.
Can 2205 clad plate be post-weld heat treated?
Yes, but the PWHT must be qualified. Long holds in the intermetallic range can form sigma phase. Order simulated PWHT (S3) and agree a test for detrimental phases, such as ASTM A923.
Which filler metals are used for SA516 Gr.70 + 2205?
Carbon steel filler for the base, a 309LMo buffer on the clad side, then 2209 duplex filler for the cap, with heat input controlled to keep the ferrite balance.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 2205 cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 2205 Duplex Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 2205 duplex stainless steel clad plate combines A240 S32205 cladding with an SA516 Grade 70 base, with 140 MPa minimum shear strength when specified and ultrasonic bond quality Class 1, 3 or 5. It is the clad choice where chloride pitting and stress corrosion cracking rule out 316L.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X