ASTM A264 SA537 Cl.1 + 316L Stainless Steel Clad Plate

ASTM A264 SA537 Cl.1 + 316L stainless steel clad plate bonds 316L stainless steel to normalized SA537 Class 1 carbon steel. The stronger, tougher base saves thickness on large high-pressure vessels in chloride service. SHH STEEL produces it by explosion bonding with shear, UT and base impact tests as ordered.
Keywords
SA537 Cl.1 + 316L clad plate, ASTM A264 316L clad plate, high strength stainless clad plate, SA537 stainless steel clad plate, 316L clad pressure vessel plate
Equivalent Grades:
ASME SA-264, GB/T 8165, NB/T 47002.1, JIS G3601; 316L = S31603 / 1.4404; SA537 Cl.1 ≈ Q370R / P355N (approx.)
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA537 Cl.1 + 316L stainless steel clad plate?

ASTM A264 SA537 Cl.1 + 316L stainless steel clad plate is a composite pressure vessel plate in which 316L (UNS S31603) austenitic stainless steel is metallurgically bonded to a normalized SA537 Class 1 carbon-manganese-silicon steel base. The steel carries the pressure; the 316L faces the process medium. It is ordered to ASTM A264 or the identical ASME SA-264.

On drawings it is written SA537 Cl.1 + 316L with a thickness pair such as 3 + 40 mm. The higher yield strength of SA537 Cl.1, 345 MPa up to 65 mm against 260 MPa for SA516 Gr.70, allows thinner walls on large, high-pressure vessels, and its normalized fine grain gives good low-temperature toughness.

It is ordered for large reactors, separators, spheres and columns in chloride-bearing petrochemical and chemical service, where the saved base thickness pays for the more expensive steel.

SHH STEEL produces 316L stainless steel clad plate by explosion bonding and supplies roll bonded clad plate where the size and thickness suit that route. We can make the common combinations used by vessel shops and heat exchanger fabricators, from thin 2 mm claddings for tanks up to thick explosion bonded plates for clad tube sheets, and we certify each plate to the ASTM A264 tests the order calls for. The wider range sits under our clad steel plates category.

ASTM A264 and ASME SA-264 at a glance

ASTM A264 is the standard specification for plate of a carbon steel or low-alloy steel base to which a layer of stainless chromium-nickel steel is integrally and continuously bonded on one or both sides. It is written mainly for pressure vessel use. ASME Section II Part A publishes the same text as SA-264; the 2023 edition of SA-264 is identical with ASTM A264-12(2019). Inch-pound values govern in the specification and SI values are conversions.

Item ASTM A264 / ASME SA-264 requirement
Scope Carbon or low-alloy steel base, stainless chromium-nickel (including duplex) cladding on one or both sides
Cladding chemistry Must meet the chemical requirements of the cladding grade in ASTM A240/A240M
Base metal Carbon or low-alloy steel to an ASTM pressure vessel plate specification, or other by agreement
Bonding process Any method that produces a plate meeting the specification; explosion bonded cladding may be made from several alloy sheets welded together
General requirements ASTM A20/A20M (base steel), ASTM A480/A480M (product analysis of the cladding)
Bond strength Shear test, 20 000 psi (140 MPa) minimum, or three bond bend tests, when the purchaser requires them
Bond integrity Visual check below 3/8 in (10 mm) total thickness; ultrasonic check to ASTM A578/A578M methods at 3/8 in (10 mm) and thicker; quality Class 1, 3 or 5
Alloy surface finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type number and the specification number

Two points cause most of the questions we receive. First, A264 does not have its own grade list. It borrows the cladding chemistry from A240 and the base steel properties from the base specification, so a complete description always names three documents. Second, the shear test and the bend test are not automatic. They apply when the purchaser specifies them, which is why the order text matters as much as the plate.

How to write the order for SA 264 material

Buyers searching for ASME SA 264 usually want to know how to order it. A clear purchase description for SA 264 material looks like this: “Clad plate to ASME SA-264, cladding SA-240 316L, 3 mm minimum; base SA-537 Class 1, normalized, 20 mm minimum; Class 1 bond quality with 100 % ultrasonic coverage (S12); shear test required; finish: pickled.” The ordering list in A264 also asks for quantity, dimensions, product analysis if needed, mechanical properties, restrictions on weld repair, corrosion testing, any construction code rules, and whether the cladding is counted in the design strength calculation or is corrosion allowance only.

SA537 Cl.1 base and 316L cladding

The base and cladding of a stainless steel clad plate are chosen for different jobs: the base for strength, toughness and code allowable stress, the cladding for the corrosion duty. SA537 Cl.1 + 316L is the most ordered pairing in petrochemical and chemical vessel work because both halves are well known to every fabricator and inspector.

SA537 Class 1 as the base steel

ASME SA537 Class 1 is a normalized carbon-manganese-silicon pressure vessel plate. Up to 65 mm it must reach 485 to 620 MPa tensile strength and 345 MPa minimum yield, against 260 MPa for SA516 Grade 70; from 65 to 100 mm, the maximum thickness for Class 1, the levels are 450 to 585 MPa and 310 MPa. Normalizing is mandatory and gives a fine-grained, tough steel that is routinely Charpy tested at low temperatures.

As a clad plate base, SA537 Cl.1 is chosen when a higher allowable stress will save real thickness on large or high-pressure vessels, when low-temperature toughness is needed, or when the owner’s standard calls for it for spheres and large storage vessels.

Why 316L is the most requested cladding

316L (UNS S31603) adds 2 to 3 % molybdenum to the 18-8 austenitic base, which raises resistance to pitting and crevice attack in chloride-bearing media compared with 304L. The low carbon content, 0.030 % maximum, limits chromium carbide precipitation during the heat cycles that a clad plate sees: bonding, flattening, stress relief and later post-weld heat treatment of the vessel. That matters more for clad plate than for solid sheet, because the base steel often has to be heat treated and the cladding goes along for the ride. The cladding chemistry is taken from ASME SA240 316L plate.

Explosion bonded vs roll bonded clad plate

Explosion bonded clad plate and roll bonded clad plate are the two main manufacturing routes; both produce a metallurgical bond that meets ASTM A264, but they suit different sizes, thicknesses and order quantities. A264 accepts any process that meets its tests, so the choice is technical and commercial rather than a matter of compliance.

Explosion bonding (explosion welding)

In explosion bonding, the 316L cladding plate is set above the SA537 base plate with a controlled stand-off gap, and a layer of explosive is spread over the cladding. The detonation travels across the plate and drives the cladding into the base at an oblique angle. At the collision point the surface films are jetted away and the clean metals bond in the solid state. The interface usually shows a regular wave pattern, and there is no bulk melting and no dilution of the 316L layer.

After bonding, the plate is flattened, inspected ultrasonically, and cut, ground or pickled to the ordered finish. Explosion bonding handles thick base steels, thick claddings and combinations that cannot be rolled, which is why it is the normal route for clad tube sheets, heavy shell courses and short project quantities. The clad plate manufacturing process also allows the cladding to be built from several 316L sheets welded together before bonding, as A264 permits, when the plate is wider than the available stainless sheet.

Hot roll bonding

In roll bonding, cleaned stainless and carbon steel slabs are stacked, sealed around the edges, and hot rolled together; the reduction in the rolling mill creates the bond by diffusion under pressure. Roll bonding is efficient for large areas, thin claddings and repeated orders of the same thickness pair. It needs a plate mill and a minimum batch, and the base steel goes through the full hot rolling and heat treatment cycle together with the cladding.

Point of comparison Explosion bonded clad plate Roll bonded clad plate
Bond mechanism Solid-state collision weld, wavy interface Diffusion bond formed during hot rolling
Best suited to Thick base or cladding, tube sheets, small to medium quantities Large plates, thinner claddings, repeat volumes
Base steel condition Base plate is bought to its own specification before bonding Base steel properties result from the rolling and heat treatment of the pack
Cladding chemistry Unchanged by the process Unchanged, but the cladding sees the full hot rolling cycle
Typical delivery forms Plates, discs and blanks for tube sheets and heads Plates and wide plates
Common limits Plate area limited by the bonding site and handling Thickness pair limited by mill capability and pack design

Weld overlay is a third way to put stainless steel on carbon steel, often used on nozzles, forgings and repairs. It is not a clad plate route in the commercial sense, because the overlay is diluted with base metal and the surface needs more deposited thickness to reach full 316L chemistry.

Bonding route and the normalized SA537 Cl.1 base

SA537 Class 1 must be delivered normalized, so the bonding route matters. Explosion bonding works on plate that is already normalized and leaves the bulk of the steel unchanged, which is why we recommend it for this base, especially in thick plate. Roll bonding heats and deforms both layers; the clad plate then has to be normalized after rolling to restore the base properties, and the 316L cladding goes through the same cycle. Either way, the certificate must show the base tested in its final heat treated condition.

For plates near the 100 mm Class 1 limit, explosion bonding is the practical route, and the base mill certificate should show normalizing before cladding.

Chemical composition of 316L cladding and SA537 Cl.1 base

The chemical composition of an ASTM A264 clad plate is certified layer by layer: the 316L cladding to ASTM A240 and the SA537 Cl.1 base to ASTM A537 / ASME SA-537. The clad plate manufacturer certifies both analyses to the purchaser.

316L cladding (UNS S31603)

Element 316L cladding, heat analysis (A240), % Product analysis tolerance (A480 Table A1.1), %
Carbon (C) 0.030 max +0.005
Manganese (Mn) 2.00 max +0.04
Phosphorus (P) 0.045 max +0.010
Sulfur (S) 0.030 max +0.005
Silicon (Si) 0.75 max +0.05
Chromium (Cr) 16.0 – 18.0 ±0.20
Nickel (Ni) 10.0 – 14.0 ±0.15
Molybdenum (Mo) 2.00 – 3.00 ±0.10
Nitrogen (N) 0.10 max +0.01
Iron (Fe) Balance —

Heat analysis limits are those of A240 for UNS S31603. Product analysis is not mandatory; when the purchaser asks for it, the result is judged against the heat limits plus the A480 tolerances shown. A480 sets each tolerance by the maximum of the specified range and applies it under the minimum and over the maximum. To avoid picking up iron from the base, A264 tells the laboratory to remove all the base metal plus 40 % of the cladding from the bonded side, up to 1.6 mm, before taking millings, or to spark the centre line of the cladding when it is thick enough.

SA537 Class 1 base steel

Element SA537 Cl.1 heat analysis, % Product analysis, %
Carbon (C) 0.24 max 0.24 max
Manganese (Mn), 40 mm and under 0.70 – 1.35 0.64 – 1.46
Manganese (Mn), over 40 mm 1.00 – 1.60 0.92 – 1.72
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.50 0.13 – 0.55
Copper (Cu) 0.35 max 0.38 max
Nickel (Ni) 0.25 max 0.28 max
Chromium (Cr) 0.25 max 0.29 max
Molybdenum (Mo) 0.08 max 0.09 max

Manganese may exceed 1.35 % (up to 1.60 %) and nickel 0.25 % (up to 0.50 %) on heat analysis if the carbon equivalent CE = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15 does not exceed 0.57 %. Older editions allowed 0.035 % phosphorus and sulfur; the values shown follow the current limits, so confirm the edition on the certificate.

Mechanical properties, shear strength and bond integrity

Mechanical testing of a 316L clad steel plate covers three things: the tensile properties of the composite or of the base, the strength of the bond, and the extent of any unbonded area. Each specimen is tested in the final heat treated condition of the plate, including simulated post-weld heat treatment when that supplementary requirement is ordered.

Tensile test: composite or base steel only

Condition How tensile properties are determined Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less, base minimum yield 275 MPa or less Full-thickness test of the composite plate Not below the base steel minimum and not more than 35 MPa above the base steel maximum
Composite over 38 mm, or base minimum tensile over 485 MPa, or base minimum yield over 275 MPa Test of the base steel only (round specimen from the base for plates over 38 mm) All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

SA537 Cl.1 has a minimum yield of 345 MPa, above the 275 MPa threshold in A264, so the clad plate tensile test is made on the base steel only, whatever the total thickness, and must meet all SA537 Cl.1 requirements. 316L is weaker than the base, so including it would only lower the result; designers normally treat the cladding as corrosion allowance.

Strength of the two layers

Property 316L cladding (A240) SA537 Cl.1 base
Tensile strength 485 MPa min 485 – 620 MPa (to 65 mm); 450 – 585 MPa (over 65 to 100 mm)
Yield strength (0.2 % offset) 170 MPa min 345 MPa min (to 65 mm); 310 MPa min (over 65 to 100 mm)
Elongation 40 % min in 50 mm 22 % min in 50 mm; 18 % min in 200 mm
Hardness 217 HBW / 95 HRB max Not specified

Bond shear strength (clad plate shear test)

The clad plate shear test pushes the cladding off a machined step on the base and measures the load per unit bonded area. When the purchaser requires it, A264 sets a minimum shear strength of 20 000 psi (140 MPa). The minimum cladding thickness for the shear specimen is 1.9 mm; thinner claddings can be shear tested only by agreement. One shear test represents each plate as rolled, taken near a top or bottom corner, parallel to the longitudinal axis, or at another location representative of the final product.

Bond bend test

As an alternative to the shear test, three bend tests are made with the cladding in compression and bent through 180°. At least two of the three must show no more than 50 % separation on both edges of the bent portion. Bend specimens are taken at right angles to the longitudinal axis, 38 mm wide and not more than 19 mm thick, keeping the same clad-to-base ratio as the plate.

Ultrasonic bond integrity classes

Bond quality class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) in its longest dimension 1 % of the clad surface max
Class 3 75 mm (3 in) in its longest dimension 3 % of the clad surface max
Class 5 58 cm² (9 in²) 5 % of the clad surface max

Plates of 10 mm total minimum thickness and above are ultrasonically inspected for bond integrity using the procedures of ASTM A578/A578M; thinner plates are inspected visually, with UT only when specified. A non-bond is a complete loss of back reflection with an echo from the interface plane. Near a cut edge, indications over 50 % of the back reflection within 25 mm of the edge count as unbonded. If no class appears on the order, the manufacturer may supply Class 5, and the extent of scanning is the manufacturer’s choice unless 100 % coverage (Supplementary Requirement S12) is ordered. For tube sheets and heads we recommend stating Class 1 with 100 % coverage.

Impact testing of the SA537 Cl.1 base

Normalized SA537 Cl.1 is routinely Charpy tested at low temperatures under A20 supplementary requirements or the vessel code. On a clad plate, impact specimens are taken from the base steel only, with the cladding removed, and after any simulated PWHT ordered. State the test temperature, energy and specimen orientation on the order; the clad plate certificate then reports them with the shear and ultrasonic results.

Heat treatment and post-weld heat treatment

Heat treatment of an austenitic stainless steel clad plate under ASTM A264 is, by default, a solution treatment for the chromium carbides in the cladding followed by air cooling, unless the purchaser and manufacturer agree otherwise. Air-hardening low-alloy bases are tempered afterwards, and where the plate is made without hot rolling the two components may be heat treated separately before bonding. Duplex clad plates are delivered in a heat treated condition agreed at the order.

In daily practice the delivery condition is one of the items buyers should settle in writing. An explosion bonded SA537 Cl.1 + 316L plate is often supplied as-clad and flattened, or stress relieved, by agreement, because a full solution treatment at stainless steel temperatures would also take the carbon steel through a temperature range it was not designed for. When plates are to be cold formed, or when the base specification requires it, the purchaser may ask for normalizing of the base for grain refinement after solution annealing.

If the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the mechanical test coupons see a simulated PWHT. The low carbon of 316L is the reason it tolerates this better than 316; for long or repeated PWHT cycles, discuss intergranular corrosion testing of the cladding as an additional requirement.

SA537 Cl.1 must be in the normalized condition. Explosion bonding is done on normalized plate and is a cold process for the bulk of the steel; if the plate is renormalized after bonding, the 316L cladding goes through the same cycle, which is acceptable for low-carbon 316L. State any PWHT so coupons can be tested in that condition, including Charpy tests of the base.

Thickness tolerances and surface finish

Thickness tolerances for ASTM A264 clad plate depend on whether the plate is ordered to minimum or nominal thickness. Minimum thicknesses of the cladding, the base, or the total composite are as stated in the purchase order. When nominal thicknesses are ordered, the permitted under-tolerance is 0.3 mm for the base steel or total composite and 0.8 mm for the cladding.

Tolerance item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Ordered to nominal: base steel or total composite 0.3 mm (0.01 in) under
Ordered to nominal: cladding 0.8 mm (0.03 in) under
Over-tolerance of total composite Greater of 3 mm (0.125 in) or 10 % of the ordered total, in the base, the cladding or both, provided each minimum is met
Width, length, flatness and other variations ASTM A20/A20M
Restricted tolerances May be agreed between purchaser and manufacturer

For pressure vessel work we recommend ordering the cladding to a minimum thickness, typically 3 mm, so that the corrosion allowance in the design is guaranteed after any grinding. The 316L surface is delivered blasted, pickled, blast-cleaned and pickled, or fully conditioned, and the steel side as bonded or shot blasted. For tube sheets, the stainless face can be machined after bonding.

Stock sizes and available thickness combinations

SA537 Cl.1 + 316L stainless steel clad plate is ordered by its thickness combination, cladding plus base, followed by width and length. The combinations below are the ones fabricators ask for most often; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
3 + 25 28 Large vessel shells
3 + 30 33 Separators
3 + 40 43 High-pressure reactors
4 + 50 54 Thick shells
4 + 60 64 Heads and thick shells
5 + 65 70 Upper limit of the 485 MPa band
6 + 80 86 Thick plate, 450 MPa band
6 + 100 106 Class 1 maximum base thickness
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Size limits differ between explosion bonded and roll bonded plates, and the heaviest pairs are explosion bonded. When you enquire, give the minimum cladding thickness separately from the base thickness; a plate called “23 mm” can mean 3 + 20 or 2 + 21, and the price and test plan differ.

Clad plate welding procedure for SA537 Cl.1 + 316L

A clad plate welding procedure treats the joint as two welds: a carbon steel weld for the strength member and a stainless overlay that restores the 316L surface. The key rule is that carbon steel filler must never be deposited on the cladding, because iron dilution would leave a low-alloy, corrosion-prone strip along the seam.

  1. Prepare the joint so that the cladding is cut back slightly from the root, or bevel from the steel side, according to the qualified procedure.
  2. Weld the SA537 Cl.1 side first with a matching carbon steel filler.
  3. Back-gouge or grind from the clad side to sound carbon steel weld metal.
  4. Deposit a transition (buffer) layer with an over-alloyed filler; for 316L cladding a 309MoL type is normally used, for 304L a 309L type.
  5. Cap with 316L filler so the top layer has full 316L chemistry, then pickle and passivate the weld area.

When access is only from the steel side, the stainless part of the joint is welded with stainless fillers through the full depth from the cladding upward, and the carbon steel is completed afterward. Weld procedures and welders are qualified to ASME Section IX, which A264 also requires for any welding that is part of the delivered plate, including welded cladding assemblies and cladding repairs.

Cutting is usually by plasma from the cladding side or by oxy-fuel from the steel side for thicker plates, followed by grinding of the cut face before welding. Avoid carbon steel contamination of the 316L face during handling, rolling and forming: use clean slings, cover the stainless side, and keep carbon steel grinding discs away from it.

On the steel side, SA537 Cl.1 has a higher carbon equivalent than SA516 Gr.70 at large thickness, so preheat and heat input follow the qualified procedure; low-hydrogen E7018-1 or equivalent filler is normal, with impact-tested procedure qualifications when the design temperature requires them.

Applications of 316L stainless steel clad plate

316L stainless steel clad plate is used wherever a pressure-retaining carbon steel shell needs a corrosion-resistant inner face and solid stainless steel would be heavier or more expensive than needed. The thicker the shell, the stronger the case for clad plate.

  • Large reactors and separators in chloride-bearing petrochemical service.
  • Columns where wall thickness is set by pressure and wind load.
  • Spheres and large storage vessels specified with SA537 by the owner.
  • Cold-climate outdoor vessels needing low-temperature impact tests.
  • Heat exchanger shells and channels of large diameter.
  • Refinery high-pressure vessels with sour or chloride process streams.

Why SA537 Cl.1 as the base

SA537 Cl.1 makes sense when design stress sets the wall: its higher allowable stress reduces base thickness, weight and welding time on large vessels, and normalized fine-grain steel gives the impact toughness that cold-climate and low-temperature duties need.

For moderate pressure and ordinary temperatures, SA516 Gr.70 + 316L is cheaper and more widely stocked.

The case for SA537 Cl.1 grows with vessel size: on a thick shell, every millimetre of base saved also cuts welding consumables, PWHT furnace load and transport weight, while the 316L layer stays the same. On small vessels the saving rarely covers the higher plate price and the normalizing step.

Testing and certification

Testing and certification of ASTM A264 clad plate combines the base steel tests, the bond tests and the cladding chemistry in one report. Each plate is identified so that the test results trace to it.

Test or document Basis Frequency / note
Chemical analysis of base and cladding A537 / A240, certified by the clad plate manufacturer Each heat; product analysis if ordered
Tensile test A264 Section 7 and the base steel specification Per base specification, each plate as rolled
Shear test or three bond bend tests A264 7.2 When specified; one shear test or three bend tests per plate
Ultrasonic bond inspection A578/A578M procedures; Class 1, 3 or 5 Plates 10 mm and thicker; 100 % coverage with S12
Charpy V-notch impact test Supplementary Requirement S5 When ordered for the base steel
Simulated PWHT of test coupons Supplementary Requirement S3 When the vessel will be heat treated
Liquid penetrant examination of cladding repairs A264 Section 14 Each weld repair, with location and procedure reported
Visual and dimensional inspection A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Repairs to the cladding by welding are allowed under A264 when the defect is removed and checked by liquid penetrant, the repair uses a procedure suitable for the cladding, the surface is restored, and the repair details are reported in the certificate. If your project does not accept cladding repairs, or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards cover the same product, a stainless layer bonded to a pressure vessel steel, but each sets its own test levels; use the table to cross-check a specification, not to substitute one for another without review.

Standard Title / scope Bond shear requirement Bond quality levels
ASTM A264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
ASME SA-264 ASME Code adoption of A264 Same as A264 Same as A264
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plates for pressure equipment, Part 1: stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
EN 13445-2 Material rules for unfired pressure vessels, including clad steels Per project specification Per project specification

The cladding and base grades also have equivalents in other systems. These are close, not identical, substitutes and must be checked against the design code.

Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 316L S31603 1.4404 (X2CrNiMo17-12-2) SUS316L 022Cr17Ni12Mo2 (S31603)
Base A537 / SA-537 Class 1 K12437 P355N (approx.) SPV355 (approx.) Q370R (approx.)

For Chinese pressure equipment the nearest product is GB/T 8165 or NB/T 47002.1 S31603 on Q370R; in Japan, JIS G3601 SUS316L on SPV355. These are close, not exact; check them against the design code.

Why order clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying pressure vessel shops, EPC contractors and heat exchanger builders. What buyers tell us they value is not a long list of claims but a short list of habits: For SA537 Cl.1 orders we confirm the normalizing route and the Charpy test temperature of the base before production.

  • We read the order against ASTM A264 before quoting and point out missing items, such as the bond class, the shear test or the PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • We supply cladding and base steel with traceable mill certificates, and the clad plate report with UT maps when 100 % coverage is ordered.
  • We can cut tube sheet discs and head blanks so the plate arrives ready for the next step.

FAQ

Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A; the 2023 SA-264 is identical with ASTM A264-12(2019). Use SA-264 for ASME Code vessels and state the edition if your code requires it.
What shear strength does an ASTM A264 clad plate need?
When the purchaser specifies the clad plate shear test, the minimum is 20 000 psi (140 MPa), one test per plate as rolled. The alternative is three bond bend tests through 180°, with at least two showing no more than 50 % edge separation.
Why choose SA537 Cl.1 rather than SA516 Gr.70 as the base?
SA537 Cl.1 is normalized and has 345 MPa minimum yield up to 65 mm against 260 MPa, so it saves thickness on high-pressure vessels and gives better low-temperature toughness.
Which ultrasonic class should I specify for 316L clad steel plate?
Class 1 is the tightest: no unbonded area over 25 mm and no more than 1 % in total. It is the usual choice for tube sheets and heads. If no class is ordered, Class 5 may be supplied, so always write the class and the coverage on the order.
What filler metals are used to weld SA537 Cl.1 + 316L?
A carbon steel filler for the base, a 309MoL type transition layer over the carbon steel weld on the clad side, and a 316L cap. Carbon steel filler must not touch the cladding. Procedures are qualified to ASME Section IX.
What is the HS code for stainless steel clad plate?
The clad plate HS code depends on the base steel and width. Clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. Narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
Send the clad plate standard (ASTM A264 or ASME SA-264), cladding grade and minimum thickness, base grade and thickness, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish, certificate type and destination.

Request a quotation for ASTM A264 SA537 Cl.1 + 316L Stainless Steel Clad Plate

ASTM A264 SA537 Cl.1 + 316L stainless steel clad plate combines a 316L cladding to A240 with an SA537 Class 1 base, bonded by explosion or roll bonding, with a 140 MPa minimum shear strength when specified and ultrasonic bond quality Class 1, 3 or 5.

Send the thickness combination, plate size or drawing, quantity, test requirements and certificate type to SHH STEEL. Compare other standards on our stainless steel clad plates page. Availability, testing and delivery are confirmed against each enquiry.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X