ASTM A264 SA516 Gr.70 + 317L Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 317L stainless steel clad plate bonds a 3 to 4 % molybdenum, low-carbon stainless layer to a carbon steel pressure vessel base. It handles chlorides and acids beyond the reach of 316L, in FGD, pulp bleaching and chemical service. SHH STEEL produces it by explosion or roll bonding with shear and ultrasonic tests.
Keywords
317L stainless steel clad plate, ASTM A264 317L clad plate, SA516 Gr.70 + 317L, S31703 clad plate, 317L clad steel plate
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 317L = S31703 / 1.4438
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 317L stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 317L stainless steel clad plate is a bimetal pressure vessel plate made of a 317L (UNS S31703) high-molybdenum low-carbon austenitic stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 317L face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

It is written SA516 Gr.70 + 317L with the thickness pair, such as 3 + 20 mm. 317L is the next step up from 316L: about one more percent of molybdenum, two more of chromium and more nickel, with carbon still held to 0.030 %. That moves the cladding into media where 316L pits or corrodes too quickly, while staying far cheaper than 904L or nickel alloys.

Engineers typically specify 317L clad plate for flue gas desulfurization equipment, pulp bleach plants and acid processes with chloride contamination, where 316L is marginal and a full nickel alloy would be overspending.

SHH STEEL can produce 317L clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 317L clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 317L
Cladding A240 / SA-240 317L, UNS S31703
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A complete order line reads: “Clad plate to ASME SA-264, cladding SA-240 Type 317L, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1 bond quality, 100 % UT (S12); shear test required.” For FGD and bleach plant equipment, add the corrosion test the owner’s specification requires.

SA516 Gr.70 base and 317L cladding

The two layers of SA516 Gr.70 + 317L are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 317L for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 317L is specified as the cladding

317L (ASME SA240 317L) contains 18.0 to 20.0 % chromium, 11.0 to 15.0 % nickel and 3.0 to 4.0 % molybdenum. Its pitting resistance equivalent number is about 28 at minimum chemistry, against about 23 for 316L. In practice that means better resistance to pitting and crevice corrosion in chloride solutions and better performance in sulfuric, acetic and formic acids with halide contamination.

The low carbon matters as much as the molybdenum. A clad plate goes through bonding, flattening, stress relief and the vessel’s PWHT; a carbon limit of 0.030 % keeps the cladding resistant to sensitization through all of them. Note that A240 sets the same 515/205 MPa minimum strength for 317L as for 316.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

317L compared with neighbouring claddings

Cladding Mo, % Approx. PREN (min. chemistry) Choose it when
316L (S31603) 2.00 – 3.00 23 Moderate chlorides, mild acids
317L (S31703) 3.0 – 4.0 28 FGD, bleach plants, contaminated acids
904L (N08904) 4.0 – 5.0 32 Sulfuric acid, stronger chlorides
254SMO (S31254) 6.0 – 6.5 42 Seawater and severe chlorides

Explosion bonded and roll bonded 317L clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 317L plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

317L bonds by explosion or rolling like other austenitic grades. Most 317L clad plate for FGD absorbers is supplied in 2 to 3 mm claddings on 10 to 20 mm steel, where roll bonding is economical; heavier sections are explosion bonded.

Chemical composition of 317L cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 317L clad plate is certified layer by layer: the 317L cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

317L cladding (UNS S31703)

Element 317L cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.030 max 0.005 over max ≤ 0.035
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.045 max 0.010 over max ≤ 0.055
Sulfur (S) 0.030 max 0.005 over max ≤ 0.035
Silicon (Si) 0.75 max 0.05 over max ≤ 0.80
Chromium (Cr) 18.0–20.0 0.20 under min / 0.20 over max 17.80–20.20
Nickel (Ni) 11.0–15.0 0.15 under min / 0.15 over max 10.85–15.15
Molybdenum (Mo) 3.0–4.0 0.10 under min / 0.10 over max 2.90–4.10
Nitrogen (N) 0.10 max 0.01 over max ≤ 0.11
Iron (Fe) Balance — —

These are the A240 limits for UNS S31703, with the A480 product analysis tolerances. Watch two lines on the certificate: carbon, which must stay at 0.035 % or below on product analysis, and molybdenum, which must stay at 2.90 % or above.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 317L clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 317L cladding (A240) SA516 Gr.70 base
Tensile strength 515 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 205 MPa min 260 MPa min
Elongation 40 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 217 HBW / 95 HRBW max Not specified

A 3 + 20 mm SA516 Gr.70 + 317L plate is tested full thickness, with the composite between 485 and 655 MPa. 317L is slightly stronger than 316L, so the composite results usually sit near the middle of the range.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. FGD absorber shells are commonly ordered Class 3; heads and tube sheets Class 1 with 100 % coverage.

Heat treatment of SA516 Gr.70 + 317L clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

317L clad plate is normally delivered as-clad and flattened or stress relieved by agreement. Its low carbon allows the base steel’s stress relief and PWHT without serious sensitization.

High-molybdenum austenitic grades can form intermetallic phases after long exposure at intermediate temperatures. Normal PWHT cycles are short enough not to matter, but if repeated cycles are planned, qualify them on S3 coupons and consider a corrosion test.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 317L cladding to a minimum thickness, typically 2 or 3 mm. The 317L face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 317L clad plate

SA516 Gr.70 + 317L clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 317L; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 8 10 Light tanks
2 + 10 12 Storage tanks
3 + 10 13 Low-pressure vessels
3 + 12 15 Vessel shells and heads
3 + 14 17 Process vessels
3 + 16 19 Columns, absorbers
3 + 20 23 Reactors, exchanger shells
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Small tube sheets
6 + 50 56 Tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 317L clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 317L surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309MoL type filler, which carries molybdenum into the first layer.
  5. Cap with 317L filler (ER317L), or a higher-alloy filler where the weld must out-perform the plate, then pickle and passivate the weld zone.

Weld metal of matching composition can be slightly less resistant to pitting than the wrought plate because molybdenum segregates during solidification. For critical FGD and bleach service, some owners specify an over-alloyed cap, for example a nickel-base filler, on 317L cladding.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 317L stainless steel clad plate

317L stainless steel clad plate is used where 316L is not quite enough and a nickel alloy would be too costly.

  • Flue gas desulfurization: absorber shells, spray zones and outlet ducts.
  • Pulp and paper: chlorine dioxide bleach towers and washers.
  • Chemical processing: acetic, formic and sulfuric acid service with halides.
  • Textile and dye plants with acidic chloride liquors.
  • Condensers and coolers on brackish water.
  • Pharmaceutical reactors with chloride-bearing media.

317L or 904L?

904L has more nickel, molybdenum and copper and is the better choice for sulfuric acid. 317L costs less and is often sufficient for chloride-contaminated process streams and FGD. Plant corrosion data, or a coupon test, should decide.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 317L Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Pitting or intergranular corrosion test of cladding ASTM G48 or A262 practice, by agreement FGD and bleach service; when ordered
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 317L, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 317L UNS S31703 1.4438 (X2CrNiMo18-15-4) SUS317L 022Cr19Ni13Mo3 (S31703)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Japanese projects order the same plate to JIS G3601 with SUS317L cladding; Chinese projects use GB/T 8165 or NB/T 47002.1 with S31703. Equivalents are close, not identical; check them against the design code.

Why order 317L clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 317L orders, often FGD and bleach plant equipment, we confirm the corrosion test and filler choice before production.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

What is the difference between 317L and 316L clad plate?
317L has 3.0 to 4.0 % molybdenum, 18 to 20 % chromium and 11 to 15 % nickel, against 2 to 3 %, 16 to 18 % and 10 to 14 % for 316L. It resists pitting and acid attack better and has a higher minimum yield (205 vs 170 MPa).
Where is 317L clad plate used?
Mainly in flue gas desulfurization absorbers, pulp bleach plants and chemical vessels with chloride-contaminated acids.
Which filler metals weld SA516 Gr.70 + 317L?
Carbon steel filler for the base, a 309MoL buffer and a 317L or over-alloyed cap on the clad side.
Can 317L clad plate be stress relieved?
Yes. Its 0.030 % maximum carbon limits sensitization during the base steel's stress relief and PWHT.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 317L cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 317L Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 317L stainless steel clad plate combines an A240 317L layer with 3 to 4 % molybdenum and an SA516 Grade 70 base, with 140 MPa shear strength when specified and ultrasonic Class 1, 3 or 5. It is the economical step up from 316L for FGD, bleach plant and contaminated acid service.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *