ASME SB-265 Grade 9 Titanium Plate | Ti-3Al-2.5V (UNS R56320)
What is ASME SB-265 Grade 9 titanium plate?
ASME SB-265 Grade 9 titanium plate is made to ASME SB-265, the ASME Boiler and Pressure Vessel Code Section II, Part B specification for titanium and titanium alloy strip, sheet and plate. It carries the UNS number R56320. Grade 9 is Ti-3Al-2.5V, sometimes called half 6-4. It is a near-alpha / alpha-beta alloy with about 50% more strength than Grade 2, while remaining more formable and weldable than Grade 5.
This alloy sits between commercially pure titanium and Ti-6Al-4V. Its aluminium and vanadium contents are lower than Ti-6Al-4V, so it has a mostly alpha structure with a little beta phase. It gives substantially more strength than CP titanium while remaining weldable and more cold formable than Ti-6Al-4V, and it is normally used annealed.
Its typical density of about 4.48 g/cm³ is a little over half that of carbon steel, which is one reason titanium plate is chosen where weight matters.
Because SB-265 adopts ASTM B265, it uses the same grade numbers and UNS numbers. A grade being listed in SB-265 does not by itself mean it has allowable stresses for every Code; that depends on Section II, Part D and the Code of construction.
SHH STEEL handles Grade 9 plate enquiries within its range of titanium alloy plates and sheets, checking the ordered ASME SB-265 edition, product form and certificate type before confirming supply. Related designations covered on this site include ASTM B265 Grade 9, JIS H4600 Class 61 TAP3250, GB/T 3621 TA18.
Material specification for ASME SB-265 Grade 9
ASME SB-265 is the specification for titanium and titanium alloy strip, sheet and plate in ASME Boiler and Pressure Vessel Code Section II, Part B. It adopts ASTM B265 with any ASME changes noted on its cover, so the product definitions and test requirements follow the adopted B265 edition.
| Ordering item | ASME SB-265 basis |
|---|---|
| Specification | ASME SB-265 in the BPVC Section II, Part B edition named by the Code of construction |
| Grade / UNS | Grade 9, Ti-3Al-2.5V, UNS R56320 |
| Product forms | Plate over 0.187 in (4.75 mm) and over 10 in (254 mm) wide; sheet and strip 0.187 in (4.75 mm) and under |
| Condition | Annealed |
| Code use | Allowable stresses, if any, come from Section II, Part D for the Code and edition being used |
| Certificate | Manufacturer’s report certifying SB-265; add ASTM B265 if dual certification is needed |
| Marking | Specification number, grade, heat number, manufacturer’s identification and nominal thickness |
The ASME edition referenced by a design may lag the newest ASTM B265 edition. If the plate will be stamped or used for Code construction, state SB-265, the Section II edition and any Code Case on the order, and confirm that the grade is accepted for the intended Code before design is fixed.
Chemical composition of ASME SB-265 Grade 9 (UNS R56320)
Single values are maximums; ranges are shown where an element is added. Titanium is the remainder. The product analysis column applies to check analysis on finished product.
| Element | Heat analysis, % | Permissible variation in product analysis, % |
|---|---|---|
| Nitrogen (N) | 0.03 | +0.02 |
| Carbon (C) | 0.08 | +0.02 |
| Hydrogen (H) | 0.015 | +0.002 |
| Iron (Fe) | 0.25 | +0.15 |
| Oxygen (O) | 0.15 | +0.03 |
| Aluminium (Al) | 2.5–3.5 | ±0.40 |
| Vanadium (V) | 2.0–3.0 | ±0.15 |
| Other elements, each | 0.1 | +0.02 |
| Other elements, total | 0.4 | — |
| Titanium (Ti) | Balance | — |
The heat is analysed for the listed elements and hydrogen is reported on the final product. Residual elements need not be reported unless they exceed the each or total limits. Because SB-265 adopts B265, the limits match the ASTM grade in the adopted edition.
Mechanical properties of ASME SB-265 Grade 9
The values below are the requirements for Grade 9 plate in the annealed condition.
| Property | Requirement |
|---|---|
| Tensile strength, min | 90 ksi (620 MPa) |
| Yield strength, 0.2% offset | 70 ksi (483 MPa) min |
| Elongation in 2 in or 50 mm, min | 15% |
| Bend test, under 0.070 in (1.8 mm) | Mandrel radius 2.5T, bent 105° without outside fracture |
| Bend test, 0.070–0.187 in (1.8–4.75 mm) | Mandrel radius 3T |
| Bend test, over 0.187 in (4.75 mm) | Not applicable to material over 4.75 mm |
Tensile tests are made at room temperature. Only a minimum yield strength is set for this grade. Bend tests apply to sheet and strip up to 0.187 in (4.75 mm); plate over that thickness is not bend tested under the specification.
Elevated-temperature design values are not part of the plate specification. They come from the design code, such as ASME Section II, Part D where the grade is listed.
Delivery condition, finish and marking
ASME SB-265 covers material in the annealed condition. Plate must be free of injurious external and internal imperfections. Annealed product may be furnished descaled, sandblasted, ground, or sandblasted and ground; state the finish on the order.
- Condition: Annealed
- Surface: descaled, sandblasted or ground, as ordered; minor spot grinding is permitted within the thickness tolerance
- Marking: specification, grade, heat number, manufacturer’s identification and nominal thickness, in rows that can be removed with hot alkaline cleaning
- Packaging: boxed, crated, boarded or as the manufacturer’s standard practice unless the order states otherwise
The alloy is supplied annealed; it is not normally strengthened by heat treatment in plate form. If the plate will be formed or welded in your shop, say so at enquiry so the finish and protective packing suit the next process.
Welding and fabrication of Grade 9 titanium plate
Grade 9 welds readily by gas tungsten arc, plasma arc, electron beam and laser processes with full inert-gas shielding.
- Use trailing shields and back purging until the weld cools below about 400 °C
- Use matching or engineer-approved filler metal
- Clean joints and filler wire, and keep carbon steel tools away from the surface
- Use weld colour as a check of shielding quality
Cold forming is possible with larger bend radii than for CP grades. Severe shapes may need warm forming.
Machining is easier than for Ti-6Al-4V but still needs sharp tools, low cutting speeds, steady feeds and generous coolant. Heat stays at the cutting edge because titanium conducts heat poorly, so avoid dwelling and keep fine chips away from ignition sources.
These are general practices, not a qualified procedure. The fabricator must qualify the welding procedure, filler metal and inspection to the applicable code.
Dimensional tolerances and flatness
Dimensional tolerances are set in the specification’s tables for thickness, width, length, weight and flatness. Plate flatness has its own table for annealed plate. For sheet, cold-rolled tolerances apply unless hot-rolled sheet is ordered.
State the nominal thickness, width, length, quantity and any cutting drawing at enquiry. If a project needs tighter flatness, a specific edge condition or cut-to-size pieces, write it on the order rather than relying on the default tables. No stock sizes are implied by this page.
Titanium plate can be cut by waterjet, abrasive saw, plasma or machining. Thermal cutting leaves an oxygen-enriched edge that should be removed by machining or grinding before welding or forming, so agree the cut-edge condition and any machining allowance on the order.
Applications and service limits of Grade 9 titanium plate
Typical uses of Grade 9 plate include:
- Lightweight sheet structures and ducting
- Pressure and hydraulic system parts made from plate
- Sporting goods and bicycle components
- Welded assemblies needing more strength than CP titanium with better formability than Ti-6Al-4V
It is not a direct substitute for Grade 5 where full 6-4 strength is required. The alloy is not suited to hydrofluoric acid, fluoride-bearing media, dry chlorine or red fuming nitric acid. In hot reducing brines the Pd- or Ru-bearing variants are often preferred. The design engineer must confirm suitability for the actual medium and temperature.
When selecting Grade 9, compare it with Grade 18, Grade 28, Grade 40. The choice usually turns on the balance of strength, formability, corrosion behaviour in the actual medium and cost, and on which standard the drawing or design code names.
Compare Grade 9 with other ASME SB-265 grades
The grades below are the closest neighbours of Grade 9 in ASME SB-265. Values are tensile strength, 0.2% yield or proof strength and minimum elongation, as set by the standard.
| Grade | Tensile strength | Yield / proof strength | Elongation, min | Typical role |
|---|---|---|---|---|
| Grade 9 (R56320) | 90 ksi (620 MPa) | 70 ksi (483 MPa) min | 15% | Half-strength 6-4, good formability |
| Grade 18 (R56322) | 90 ksi (620 MPa) | 70 ksi (483 MPa) min | 15% | Ti-3Al-2.5V with Pd |
| Grade 28 (R56323) | 90 ksi (620 MPa) | 70 ksi (483 MPa) min | 15% | Ti-3Al-2.5V with Ru |
| Grade 40 (R54407) | 95 ksi (655 MPa) | 75 ksi (517 MPa) min | 15% | Ti-3.9V-0.85Al-0.25Fe-0.25Si |
Grades in this group share a similar base alloy; differences come from precious-metal additions or alloy balance. Confirm the strength and corrosion needs before changing grade.
ASME SB-265 Grade 9 equivalent grades
The designations below are commonly compared with ASME SB-265 Grade 9. They are close in composition and role, but limits, tests and product forms are set by each standard, so they are not automatically interchangeable.
| Standard / system | Designation | Relationship to ASME SB-265 Grade 9 |
|---|---|---|
| ASTM B265 | Grade 9 | ASTM specification adopted by SB-265; same grade requirements |
| JIS H4600 | Class 61 (TAP3250) | Close equivalent; JIS strength range and tests differ |
| GB/T 3621 | TA18 | Close equivalent; confirm grade name and limits in the ordered edition |
| JIS H4600 | Class 61F (TAP3250F) | Nearest by role only; composition and properties differ |
| UNS | R56320 | Same unified number as ASTM Grade 9 |
| DIN / EN material number | 3.7195 (TiAl3V2.5) | Close equivalent |
Where a drawing names one designation and the supplier offers another, agree in writing which standard governs chemistry, tensile values, testing and marking. Dual or multiple certification is possible only when the material meets every cited standard in full, and the certificate must show the results against each one.
Why choose SHH STEEL for Grade 9 titanium plate
SHH STEEL supports specification-led purchasing of titanium plate and sheet.
- We quote to ASME SB-265 and the Section II edition you name, and can arrange dual SB-265 / B265 certification
- Certificates are checked against the Grade 9 chemistry and tensile limits before shipment
- Sizes, quantities, testing and delivery are confirmed in the quotation, not assumed
- Finish, marking and packing are agreed before production
Questions on equivalents, dual certification or edition changes are answered before an order is placed.
How to enquire for ASME SB-265 Grade 9 plate
Send the material schedule with the details below. We review the enquiry and raise any open points before confirming the supply route.
| Enquiry item | Information required |
|---|---|
| Material | ASME SB-265 Grade 9 (UNS R56320), Section II edition; add ASTM B265 if dual certification |
| Product form | Plate, sheet or strip; for sheet, cold or hot rolled |
| Dimensions | Thickness, width, length, quantity and any cutting drawing |
| Finish | Descaled, sandblasted, ground or other agreed surface |
| Testing | Any special mechanical properties, extra analysis or reports |
| Documents | Certificate type and any third-party inspection |
| Destination | Delivery place and packing requirements |
FAQ
-
What is the difference between ASME SB-265 Grade 9 and ASTM B265 Grade 9?
- SB-265 adopts B265, so chemistry and tensile requirements normally match the adopted edition. SB-265 is the document cited by ASME Code construction; B265 is the ASTM industrial specification. Dual certification covers both.
-
What is the tensile strength of ASME SB-265 Grade 9 titanium plate?
- The requirement is 90 ksi (620 MPa) minimum. The 0.2% proof or yield strength is 70 ksi (483 MPa) minimum. Minimum elongation is 15%. Values apply to the condition and thickness range stated in the standard.
-
What is Grade 9 mainly used for?
- Typical uses include lightweight sheet structures and ducting, pressure and hydraulic system parts made from plate and sporting goods and bicycle components. It is not a direct substitute for Grade 5 where full 6-4 strength is required.
-
Does SB-265 use the same plate, sheet and strip definitions as B265?
- Yes. Plate is over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide; thinner product is sheet if 24 in (610 mm) or more wide, otherwise strip.
-
What should I send for a quotation?
- Send ASME SB-265 Grade 9, the edition, product form, thickness, width, length and quantity, the finish, any special testing, the certificate type and the destination.
Request a quotation for ASME SB-265 Grade 9 titanium plate
ASME SB-265 Grade 9 is Ti-3Al-2.5V titanium alloy, UNS R56320, specified for 90 ksi (620 MPa) minimum tensile strength, 70 ksi (483 MPa) minimum yield or proof strength and 15% minimum elongation in the annealed condition. Typical uses include lightweight sheet structures and ducting and pressure and hydraulic system parts made from plate.
Send the product form, sizes, quantity, finish, certificate type and destination to SHH STEEL. Compare other grades on the ASME SB-265 page or browse all titanium alloy plates and sheets. Availability, testing and delivery are confirmed against each enquiry.
Contact: admin@steelspecs.com