ASTM B265 Grade 9 Titanium Plate | Ti-3Al-2.5V (UNS R56320)
What is ASTM B265 Grade 9 titanium plate?
ASTM B265 Grade 9 titanium plate is made to ASTM B265, the ASTM specification for titanium and titanium alloy strip, sheet and plate. It carries the UNS number R56320. Grade 9 is Ti-3Al-2.5V, sometimes called half 6-4. It is a near-alpha / alpha-beta alloy with about 50% more strength than Grade 2, while remaining more formable and weldable than Grade 5.
This alloy sits between commercially pure titanium and Ti-6Al-4V. Its aluminium and vanadium contents are lower than Ti-6Al-4V, so it has a mostly alpha structure with a little beta phase. It gives substantially more strength than CP titanium while remaining weldable and more cold formable than Ti-6Al-4V, and it is normally used annealed.
Its typical density of about 4.48 g/cm³ is a little over half that of carbon steel, which is one reason titanium plate is chosen where weight matters.
ASTM B265 groups its grades into unalloyed titanium, corrosion-resistant grades with small additions of palladium, ruthenium, nickel or molybdenum, and structural alloys such as Ti-3Al-2.5V and Ti-6Al-4V. Each grade has its own UNS number, and the H grades add a higher guaranteed tensile strength for pressure vessel use.
SHH STEEL handles Grade 9 plate enquiries within its range of titanium alloy plates and sheets, checking the ordered ASTM B265 edition, product form and certificate type before confirming supply. Related designations covered on this site include ASME SB-265 Grade 9, JIS H4600 Class 61 TAP3250, GB/T 3621 TA18.
Material specification for ASTM B265 Grade 9
ASTM B265 classifies flat titanium products by thickness and width. The same chemistry and tensile requirements apply to strip, sheet and plate, but dimensional tolerances and bend testing differ by product form.
| Ordering item | ASTM B265 basis |
|---|---|
| Standard | ASTM B265, Titanium and Titanium Alloy Strip, Sheet, and Plate; state the edition on the order |
| Grade / UNS | Grade 9, Ti-3Al-2.5V, UNS R56320 |
| Plate | Over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide |
| Sheet | 0.187 in (4.75 mm) and under, 24 in (610 mm) wide or more; state cold or hot rolled |
| Strip | 0.187 in (4.75 mm) and under, less than 24 in (610 mm) wide |
| Condition | Annealed |
| Certificate | Manufacturer’s report with chemical analysis, tensile results and other required tests |
Order information listed by the specification includes grade, product limitations, special mechanical properties, marking, finish, packaging, any additional reports and the disposition of rejected material. For ASME Code construction, order to ASME SB-265 Grade 9 and state any dual certification on the purchase order.
Chemical composition of ASTM B265 Grade 9 (UNS R56320)
Single values are maximums; ranges are shown where an element is added. Titanium is determined by difference. Product analysis tolerances cover variation between laboratories and do not broaden the heat analysis limits.
| Element | Heat analysis, % | Permissible variation in product analysis, % |
|---|---|---|
| Nitrogen (N) | 0.03 | +0.02 |
| Carbon (C) | 0.08 | +0.02 |
| Hydrogen (H) | 0.015 | +0.002 |
| Iron (Fe) | 0.25 | +0.15 |
| Oxygen (O) | 0.15 | +0.03 |
| Aluminium (Al) | 2.5–3.5 | ±0.40 |
| Vanadium (V) | 2.0–3.0 | ±0.15 |
| Other elements, each | 0.1 | +0.02 |
| Other elements, total | 0.4 | — |
| Titanium (Ti) | Balance | — |
Ingot top and bottom are analysed for the listed elements. Hydrogen is tested and reported on at least one final product sample, and a lower hydrogen limit may be negotiated. Other elements need not be reported unless they exceed 0.10% each or 0.40% total, and they may not be added intentionally.
Mechanical properties of ASTM B265 Grade 9
The values below are the requirements for Grade 9 plate in the annealed condition.
| Property | Requirement |
|---|---|
| Tensile strength, min | 90 ksi (620 MPa) |
| Yield strength, 0.2% offset | 70 ksi (483 MPa) min |
| Elongation in 2 in or 50 mm, min | 15% |
| Bend test, under 0.070 in (1.8 mm) | Mandrel radius 2.5T, bent 105° without outside fracture |
| Bend test, 0.070–0.187 in (1.8–4.75 mm) | Mandrel radius 3T |
| Bend test, over 0.187 in (4.75 mm) | Not applicable to material over 4.75 mm |
Tensile tests are made at room temperature. Only a minimum yield strength is set for this grade. Bend tests apply to sheet and strip up to 0.187 in (4.75 mm); plate over that thickness is not bend tested under the specification.
Elevated-temperature design values are not part of the plate specification. They come from the design code, such as ASME Section II, Part D where the grade is listed.
Delivery condition, finish and marking
ASTM B265 covers material in the annealed condition. Plate must be free of injurious external and internal imperfections. Annealed product may be furnished descaled, sandblasted, ground, or sandblasted and ground; state the finish on the order.
- Condition: Annealed
- Surface: descaled, sandblasted or ground, as ordered; minor spot grinding is permitted within the thickness tolerance
- Marking: specification, grade, heat number, manufacturer’s identification and nominal thickness, in rows that can be removed with hot alkaline cleaning
- Packaging: boxed, crated, boarded or as the manufacturer’s standard practice unless the order states otherwise
The alloy is supplied annealed; it is not normally strengthened by heat treatment in plate form. If the plate will be formed or welded in your shop, say so at enquiry so the finish and protective packing suit the next process.
Welding and fabrication of Grade 9 titanium plate
Grade 9 welds readily by gas tungsten arc, plasma arc, electron beam and laser processes with full inert-gas shielding.
- Use trailing shields and back purging until the weld cools below about 400 °C
- Use matching or engineer-approved filler metal
- Clean joints and filler wire, and keep carbon steel tools away from the surface
- Use weld colour as a check of shielding quality
Cold forming is possible with larger bend radii than for CP grades. Severe shapes may need warm forming.
Machining is easier than for Ti-6Al-4V but still needs sharp tools, low cutting speeds, steady feeds and generous coolant. Heat stays at the cutting edge because titanium conducts heat poorly, so avoid dwelling and keep fine chips away from ignition sources.
These are general practices, not a qualified procedure. The fabricator must qualify the welding procedure, filler metal and inspection to the applicable code.
Dimensional tolerances and flatness
Dimensional tolerances are set in the specification’s tables for thickness, width, length, weight and flatness. Plate flatness has its own table for annealed plate. For sheet, cold-rolled tolerances apply unless hot-rolled sheet is ordered.
State the nominal thickness, width, length, quantity and any cutting drawing at enquiry. If a project needs tighter flatness, a specific edge condition or cut-to-size pieces, write it on the order rather than relying on the default tables. No stock sizes are implied by this page.
Titanium plate can be cut by waterjet, abrasive saw, plasma or machining. Thermal cutting leaves an oxygen-enriched edge that should be removed by machining or grinding before welding or forming, so agree the cut-edge condition and any machining allowance on the order.
Applications and service limits of Grade 9 titanium plate
Typical uses of Grade 9 plate include:
- Lightweight sheet structures and ducting
- Pressure and hydraulic system parts made from plate
- Sporting goods and bicycle components
- Welded assemblies needing more strength than CP titanium with better formability than Ti-6Al-4V
It is not a direct substitute for Grade 5 where full 6-4 strength is required. The alloy is not suited to hydrofluoric acid, fluoride-bearing media, dry chlorine or red fuming nitric acid. In hot reducing brines the Pd- or Ru-bearing variants are often preferred. The design engineer must confirm suitability for the actual medium and temperature.
When selecting Grade 9, compare it with Grade 18, Grade 28, Grade 40. The choice usually turns on the balance of strength, formability, corrosion behaviour in the actual medium and cost, and on which standard the drawing or design code names.
Compare Grade 9 with other ASTM B265 grades
The grades below are the closest neighbours of Grade 9 in ASTM B265. Values are tensile strength, 0.2% yield or proof strength and minimum elongation, as set by the standard.
| Grade | Tensile strength | Yield / proof strength | Elongation, min | Typical role |
|---|---|---|---|---|
| Grade 9 (R56320) | 90 ksi (620 MPa) | 70 ksi (483 MPa) min | 15% | Half-strength 6-4, good formability |
| Grade 18 (R56322) | 90 ksi (620 MPa) | 70 ksi (483 MPa) min | 15% | Ti-3Al-2.5V with Pd |
| Grade 28 (R56323) | 90 ksi (620 MPa) | 70 ksi (483 MPa) min | 15% | Ti-3Al-2.5V with Ru |
| Grade 40 (R54407) | 95 ksi (655 MPa) | 75 ksi (517 MPa) min | 15% | Ti-3.9V-0.85Al-0.25Fe-0.25Si |
Grades in this group share a similar base alloy; differences come from precious-metal additions or alloy balance. Confirm the strength and corrosion needs before changing grade.
ASTM B265 Grade 9 equivalent grades
The designations below are commonly compared with ASTM B265 Grade 9. They are close in composition and role, but limits, tests and product forms are set by each standard, so they are not automatically interchangeable.
| Standard / system | Designation | Relationship to ASTM B265 Grade 9 |
|---|---|---|
| ASME SB-265 | Grade 9 | ASME Code adoption of B265; ordered for pressure equipment |
| JIS H4600 | Class 61 (TAP3250) | Close equivalent; JIS strength range and tests differ |
| GB/T 3621 | TA18 | Close equivalent; confirm grade name and limits in the ordered edition |
| JIS H4600 | Class 61F (TAP3250F) | Nearest by role only; composition and properties differ |
| UNS | R56320 | Same unified number as ASTM Grade 9 |
| DIN / EN material number | 3.7195 (TiAl3V2.5) | Close equivalent |
Where a drawing names one designation and the supplier offers another, agree in writing which standard governs chemistry, tensile values, testing and marking. Dual or multiple certification is possible only when the material meets every cited standard in full, and the certificate must show the results against each one.
Why choose SHH STEEL for Grade 9 titanium plate
SHH STEEL supports specification-led purchasing of titanium plate and sheet.
- We quote to the ASTM B265 edition, grade and product form you name, and keep B265 and SB-265 requirements distinct
- Certificates are checked against the Grade 9 chemistry and tensile limits
- Sizes, quantities, testing and delivery are confirmed in the quotation, not assumed
- Finish, marking and packing are agreed before production
Questions on equivalents, dual certification or edition changes are answered before an order is placed.
How to enquire for ASTM B265 Grade 9 plate
Send the material schedule with the details below. We review the enquiry and raise any open points before confirming the supply route.
| Enquiry item | Information required |
|---|---|
| Material | ASTM B265 Grade 9 (UNS R56320), edition; add ASME SB-265 if Code use |
| Product form | Plate, sheet or strip; for sheet, cold or hot rolled |
| Dimensions | Thickness, width, length, quantity and any cutting drawing |
| Finish | Descaled, sandblasted, ground or other agreed surface |
| Testing | Any special mechanical properties, extra analysis or reports |
| Documents | Certificate type and any third-party inspection |
| Destination | Delivery place and packing requirements |
FAQ
-
Is ASTM B265 Grade 9 the same as ASME SB-265 Grade 9?
- SB-265 is the ASME Code adoption of B265, so Grade 9 requirements normally match. They are separate documents, and ASME may adopt a different edition. For Code work, order SB-265 Grade 9 or dual certification.
-
What is the tensile strength of ASTM B265 Grade 9 titanium plate?
- The requirement is 90 ksi (620 MPa) minimum. The 0.2% proof or yield strength is 70 ksi (483 MPa) minimum. Minimum elongation is 15%. Values apply to the condition and thickness range stated in the standard.
-
What is Grade 9 mainly used for?
- Typical uses include lightweight sheet structures and ducting, pressure and hydraulic system parts made from plate and sporting goods and bicycle components. It is not a direct substitute for Grade 5 where full 6-4 strength is required.
-
When is a titanium product classed as plate under B265?
- Plate is over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide. Thinner product is sheet if 24 in (610 mm) wide or more, otherwise strip.
-
What should I send for a quotation?
- Send ASTM B265 Grade 9, the edition, product form, thickness, width, length and quantity, the finish, any special testing, the certificate type and the destination. Add ASME SB-265 if the plate is for Code construction.
Request a quotation for ASTM B265 Grade 9 titanium plate
ASTM B265 Grade 9 is Ti-3Al-2.5V titanium alloy, UNS R56320, specified for 90 ksi (620 MPa) minimum tensile strength, 70 ksi (483 MPa) minimum yield or proof strength and 15% minimum elongation in the annealed condition. Typical uses include lightweight sheet structures and ducting and pressure and hydraulic system parts made from plate.
Send the product form, sizes, quantity, finish, certificate type and destination to SHH STEEL. Compare other grades on the ASTM B265 page or browse all titanium alloy plates and sheets. Availability, testing and delivery are confirmed against each enquiry.
Contact: admin@steelspecs.com