ASME SB-265 Grade 18 Titanium Plate | Ti-3Al-2.5V with Pd (UNS R56322)

ASME SB-265 Grade 18 titanium plate is Ti-3Al-2.5V with Pd titanium alloy (UNS R56322) supplied annealed. It is specified for 620 MPa minimum tensile strength, 483 MPa yield and 15% minimum elongation. Typical uses include oil and gas and geothermal equipment in hot brine. SHH STEEL reviews size, finish and certificate requirements before quoting.
Keywords
ASME SB-265 Grade 18 titanium plate, Grade 18 titanium plate, UNS R56322 plate, Ti-3Al-2.5V with Pd titanium alloy plate, ASME SB-265 titanium sheet
Equivalent Grades:
UNS R56322, ASTM B265 Gr.18, ASTM B265 Gr.9
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is ASME SB-265 Grade 18 titanium plate?

ASME SB-265 Grade 18 titanium plate is made to ASME SB-265, the ASME Boiler and Pressure Vessel Code Section II, Part B specification for titanium and titanium alloy strip, sheet and plate. It carries the UNS number R56322. Grade 18 is Grade 9 (Ti-3Al-2.5V) with 0.04–0.08% palladium. It keeps the strength of Grade 9 and adds improved crevice and reducing-acid corrosion resistance.

This alloy sits between commercially pure titanium and Ti-6Al-4V. Its aluminium and vanadium contents are lower than Ti-6Al-4V, so it has a mostly alpha structure with a little beta phase. It gives substantially more strength than CP titanium while remaining weldable and more cold formable than Ti-6Al-4V, and it is normally used annealed.

Its typical density of about 4.48 g/cm³ is a little over half that of carbon steel, which is one reason titanium plate is chosen where weight matters.

Because SB-265 adopts ASTM B265, it uses the same grade numbers and UNS numbers. A grade being listed in SB-265 does not by itself mean it has allowable stresses for every Code; that depends on Section II, Part D and the Code of construction.

SHH STEEL handles Grade 18 plate enquiries within its range of titanium alloy plates and sheets, checking the ordered ASME SB-265 edition, product form and certificate type before confirming supply. Related designations covered on this site include ASTM B265 Grade 18, ASTM B265 Grade 9.

Material specification for ASME SB-265 Grade 18

ASME SB-265 is the specification for titanium and titanium alloy strip, sheet and plate in ASME Boiler and Pressure Vessel Code Section II, Part B. It adopts ASTM B265 with any ASME changes noted on its cover, so the product definitions and test requirements follow the adopted B265 edition.

Ordering item ASME SB-265 basis
Specification ASME SB-265 in the BPVC Section II, Part B edition named by the Code of construction
Grade / UNS Grade 18, Ti-3Al-2.5V with Pd, UNS R56322
Product forms Plate over 0.187 in (4.75 mm) and over 10 in (254 mm) wide; sheet and strip 0.187 in (4.75 mm) and under
Condition Annealed
Code use Allowable stresses, if any, come from Section II, Part D for the Code and edition being used
Certificate Manufacturer’s report certifying SB-265; add ASTM B265 if dual certification is needed
Marking Specification number, grade, heat number, manufacturer’s identification and nominal thickness

The ASME edition referenced by a design may lag the newest ASTM B265 edition. If the plate will be stamped or used for Code construction, state SB-265, the Section II edition and any Code Case on the order, and confirm that the grade is accepted for the intended Code before design is fixed.

Chemical composition of ASME SB-265 Grade 18 (UNS R56322)

Single values are maximums; ranges are shown where an element is added. Titanium is the remainder. The product analysis column applies to check analysis on finished product.

Element Heat analysis, % Permissible variation in product analysis, %
Nitrogen (N) 0.03 +0.02
Carbon (C) 0.08 +0.02
Hydrogen (H) 0.015 +0.002
Iron (Fe) 0.25 +0.15
Oxygen (O) 0.15 +0.03
Aluminium (Al) 2.5–3.5 ±0.40
Vanadium (V) 2.0–3.0 ±0.15
Palladium (Pd) 0.04–0.08 ±0.005
Other elements, each 0.1 +0.02
Other elements, total 0.4 —
Titanium (Ti) Balance —

The heat is analysed for the listed elements and hydrogen is reported on the final product. Residual elements need not be reported unless they exceed the each or total limits. Because SB-265 adopts B265, the limits match the ASTM grade in the adopted edition.

Mechanical properties of ASME SB-265 Grade 18

The values below are the requirements for Grade 18 plate in the annealed condition.

Property Requirement
Tensile strength, min 90 ksi (620 MPa)
Yield strength, 0.2% offset 70 ksi (483 MPa) min
Elongation in 2 in or 50 mm, min 15%
Bend test, under 0.070 in (1.8 mm) Mandrel radius 2.5T, bent 105° without outside fracture
Bend test, 0.070–0.187 in (1.8–4.75 mm) Mandrel radius 3T
Bend test, over 0.187 in (4.75 mm) Not applicable to material over 4.75 mm

Tensile tests are made at room temperature. Only a minimum yield strength is set for this grade. Bend tests apply to sheet and strip up to 0.187 in (4.75 mm); plate over that thickness is not bend tested under the specification.

Elevated-temperature design values are not part of the plate specification. They come from the design code, such as ASME Section II, Part D where the grade is listed.

Delivery condition, finish and marking

ASME SB-265 covers material in the annealed condition. Plate must be free of injurious external and internal imperfections. Annealed product may be furnished descaled, sandblasted, ground, or sandblasted and ground; state the finish on the order.

  • Condition: Annealed
  • Surface: descaled, sandblasted or ground, as ordered; minor spot grinding is permitted within the thickness tolerance
  • Marking: specification, grade, heat number, manufacturer’s identification and nominal thickness, in rows that can be removed with hot alkaline cleaning
  • Packaging: boxed, crated, boarded or as the manufacturer’s standard practice unless the order states otherwise

The alloy is supplied annealed; it is not normally strengthened by heat treatment in plate form. If the plate will be formed or welded in your shop, say so at enquiry so the finish and protective packing suit the next process.

Welding and fabrication of Grade 18 titanium plate

Grade 18 welds readily by gas tungsten arc, plasma arc, electron beam and laser processes with full inert-gas shielding.

  • Use trailing shields and back purging until the weld cools below about 400 °C
  • Use matching or engineer-approved filler metal
  • Clean joints and filler wire, and keep carbon steel tools away from the surface
  • Use weld colour as a check of shielding quality

Cold forming is possible with larger bend radii than for CP grades. Severe shapes may need warm forming.

Machining is easier than for Ti-6Al-4V but still needs sharp tools, low cutting speeds, steady feeds and generous coolant. Heat stays at the cutting edge because titanium conducts heat poorly, so avoid dwelling and keep fine chips away from ignition sources.

These are general practices, not a qualified procedure. The fabricator must qualify the welding procedure, filler metal and inspection to the applicable code.

Dimensional tolerances and flatness

Dimensional tolerances are set in the specification’s tables for thickness, width, length, weight and flatness. Plate flatness has its own table for annealed plate. For sheet, cold-rolled tolerances apply unless hot-rolled sheet is ordered.

State the nominal thickness, width, length, quantity and any cutting drawing at enquiry. If a project needs tighter flatness, a specific edge condition or cut-to-size pieces, write it on the order rather than relying on the default tables. No stock sizes are implied by this page.

Titanium plate can be cut by waterjet, abrasive saw, plasma or machining. Thermal cutting leaves an oxygen-enriched edge that should be removed by machining or grinding before welding or forming, so agree the cut-edge condition and any machining allowance on the order.

Applications and service limits of Grade 18 titanium plate

Typical uses of Grade 18 plate include:

  • Oil and gas and geothermal equipment in hot brine
  • Corrosion-resistant pressure parts needing Grade 9 strength
  • Marine hardware
  • Chemical process components

The alloy is not suited to hydrofluoric acid, fluoride-bearing media, dry chlorine or red fuming nitric acid. In hot reducing brines the Pd- or Ru-bearing variants are often preferred. The design engineer must confirm suitability for the actual medium and temperature.

When selecting Grade 18, compare it with Grade 9, Grade 28, Grade 40. The choice usually turns on the balance of strength, formability, corrosion behaviour in the actual medium and cost, and on which standard the drawing or design code names.

Compare Grade 18 with other ASME SB-265 grades

The grades below are the closest neighbours of Grade 18 in ASME SB-265. Values are tensile strength, 0.2% yield or proof strength and minimum elongation, as set by the standard.

Grade Tensile strength Yield / proof strength Elongation, min Typical role
Grade 9 (R56320) 90 ksi (620 MPa) 70 ksi (483 MPa) min 15% Half-strength 6-4, good formability
Grade 18 (R56322) 90 ksi (620 MPa) 70 ksi (483 MPa) min 15% Ti-3Al-2.5V with Pd
Grade 28 (R56323) 90 ksi (620 MPa) 70 ksi (483 MPa) min 15% Ti-3Al-2.5V with Ru
Grade 40 (R54407) 95 ksi (655 MPa) 75 ksi (517 MPa) min 15% Ti-3.9V-0.85Al-0.25Fe-0.25Si

Grades in this group share a similar base alloy; differences come from precious-metal additions or alloy balance. Confirm the strength and corrosion needs before changing grade.

ASME SB-265 Grade 18 equivalent grades

The designations below are commonly compared with ASME SB-265 Grade 18. They are close in composition and role, but limits, tests and product forms are set by each standard, so they are not automatically interchangeable.

Standard / system Designation Relationship to ASME SB-265 Grade 18
ASTM B265 Grade 18 ASTM specification adopted by SB-265; same grade requirements
ASTM B265 Grade 9 Base grade: same chemistry, lower minimum tensile strength; H material may be dual certified
UNS R56322 Same unified number as ASTM Grade 18
GB/T 3620.1 designation TA25 (Ti-3Al-2.5V-0.05Pd) Similar nominal composition; not a GB/T 3621 plate grade

Where a drawing names one designation and the supplier offers another, agree in writing which standard governs chemistry, tensile values, testing and marking. Dual or multiple certification is possible only when the material meets every cited standard in full, and the certificate must show the results against each one.

Why choose SHH STEEL for Grade 18 titanium plate

SHH STEEL supports specification-led purchasing of titanium plate and sheet.

  • We quote to ASME SB-265 and the Section II edition you name, and can arrange dual SB-265 / B265 certification
  • Certificates are checked against the Grade 18 chemistry and tensile limits before shipment
  • Sizes, quantities, testing and delivery are confirmed in the quotation, not assumed
  • Finish, marking and packing are agreed before production

Questions on equivalents, dual certification or edition changes are answered before an order is placed.

How to enquire for ASME SB-265 Grade 18 plate

Send the material schedule with the details below. We review the enquiry and raise any open points before confirming the supply route.

Enquiry item Information required
Material ASME SB-265 Grade 18 (UNS R56322), Section II edition; add ASTM B265 if dual certification
Product form Plate, sheet or strip; for sheet, cold or hot rolled
Dimensions Thickness, width, length, quantity and any cutting drawing
Finish Descaled, sandblasted, ground or other agreed surface
Testing Any special mechanical properties, extra analysis or reports
Documents Certificate type and any third-party inspection
Destination Delivery place and packing requirements

FAQ

What is the difference between ASME SB-265 Grade 18 and ASTM B265 Grade 18?
SB-265 adopts B265, so chemistry and tensile requirements normally match the adopted edition. SB-265 is the document cited by ASME Code construction; B265 is the ASTM industrial specification. Dual certification covers both.
What is the tensile strength of ASME SB-265 Grade 18 titanium plate?
The requirement is 90 ksi (620 MPa) minimum. The 0.2% proof or yield strength is 70 ksi (483 MPa) minimum. Minimum elongation is 15%. Values apply to the condition and thickness range stated in the standard.
What is Grade 18 mainly used for?
Typical uses include oil and gas and geothermal equipment in hot brine, corrosion-resistant pressure parts needing Grade 9 strength and marine hardware. The design engineer should confirm the grade for the actual service.
Does SB-265 use the same plate, sheet and strip definitions as B265?
Yes. Plate is over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide; thinner product is sheet if 24 in (610 mm) or more wide, otherwise strip.
What should I send for a quotation?
Send ASME SB-265 Grade 18, the edition, product form, thickness, width, length and quantity, the finish, any special testing, the certificate type and the destination.

Request a quotation for ASME SB-265 Grade 18 titanium plate

ASME SB-265 Grade 18 is Ti-3Al-2.5V with Pd titanium alloy, UNS R56322, specified for 90 ksi (620 MPa) minimum tensile strength, 70 ksi (483 MPa) minimum yield or proof strength and 15% minimum elongation in the annealed condition. Typical uses include oil and gas and geothermal equipment in hot brine and corrosion-resistant pressure parts needing Grade 9 strength.

Send the product form, sizes, quantity, finish, certificate type and destination to SHH STEEL. Compare other grades on the ASME SB-265 page or browse all titanium alloy plates and sheets. Availability, testing and delivery are confirmed against each enquiry.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X