ASME SA738 Grade B Q&T C-Mn-Si vessel plate, TS 85–102 ksi, YS 60 ksi, SHH STEEL

ASME SA738 Grade B Steel Plate | SA738 Gr.B Heat-Treated Vessel Plate

ASME SA738 Grade B / ASME SA738 GR.B is quenched-and-tempered C-Mn-Si plate under ASME SA-738/SA-738M for moderate and lower temperature welded vessels. Grade B is 415 MPa yield and 585–705 MPa tensile. SHH STEEL supplies SA738 Gr.B worldwide as a global steel mill sourcing partner, with 3.1 or 3.2 certificates.
Keywords
ASME SA738 Grade B, ASME SA738 GR.B, SA738 Gr.B, SA738GRB, SA-738 Grade B, A738 Grade B, heat-treated vessel plate, containment vessel plate, SA738 Grade B supplier
Equivalent Grades:
ASTM A738 Gr B (85 ksi) / JIS — / GB Q415R (near) / EN 10028-3 P420N (near) — Material Specification: ASME SA-738 / ASTM A738 — Delivery: Quenched + Tempered (Q+T, temper ≥595℃)
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Material Comparison
Heat-Treated C-Mn-Si Vessel Service
Weldability
Heat Treatment
Delivery Condition
Dimensions
Tolerances
Supplementary Requirements
Equivalent Material Grades
Applications
Global Delivery & Markets
Why Choose SHH STEEL
FAQ
Conclusion

What is ASME SA738 Grade B Steel ?

ASME SA738 Grade B, also written ASME SA738 GR.B, is heat-treated carbon-manganese-silicon steel plate under ASME SA-738/SA-738M. The specification is identical with ASTM A738/A738M. It covers five grades — Grade A, B, C, D and E — for welded pressure vessels at moderate and lower temperature service. Grade B is the 85 ksi (585 MPa) tensile class: 415 MPa yield and 585–705 MPa tensile. Grade B shall be quenched and tempered in all thicknesses. SHH STEEL is a global steel mill sourcing partner and steel manufacturer & exporter (mill-direct, China origin) for this Grade. Plate is produced to ASME SA-738/SA-738M and shipped to buyers in the USA, Europe, Middle East and Southeast Asia.

Buyers write ASME SA738 Grade B, ASME SA738 GR.B, SA738 Gr.B, SA738GRB, SA-738 Grade B, SA 738 Gr B, A738 Grade B and ASTM A738 Gr.B. A purchase order that only says “SA738” is incomplete. This is the Grade most often searched for reactor containment and other high-toughness heat-treated carbon shells. This page is not SA516 Gr.70. It is not Grade A in the same book. Grade A is the 75 ksi class and is QT only above 65 mm. It is not SA612. It is not SA737 Grade B, even though the letters match.

The steel shall be killed. Fine austenitic grain practice follows ASME SA-20 / ASTM A20. Current practice normally limits Grade B thickness to about 100 mm. Dual marking SA738 / A738 Grade B is available. Certificates can be EN 10204 3.1 or 3.2. Company scope: global steel mill sourcing partner – SHH STEEL.

Material Specification

Specification Element Requirement SHH STEEL Compliance
Grade ASME SA738 Grade B Confirmed
Product Specification ASME SA-738/SA-738M Applied
Companion Spec ASTM A738 Grade B Dual cert available
General Requirements ASME SA-20 / ASTM A20 Applied
Steel type Killed C-Mn-Si, QT Confirmed
Strength level 85 ksi / 585 MPa min tensile class Confirmed
Heat treatment Quenched and tempered, all thicknesses Confirmed
Service idea Moderate and lower temperature vessels, containment Confirmed
Supply role Global steel mill sourcing partner SHH STEEL
Markets USA, Europe, Middle East, Southeast Asia FOB / CIF as ordered
Certification EN 10204 3.1 or 3.2 / third-party As ordered

This plate sits in pressure vessel steel plates and carbon steel plates. It does not sit with ASME SA387 Cr-Mo alloy plate or ASTM A36 steel plate structural plate.

SA-20 still governs marking, testing location, retests, repair rules and supplementary requirements unless the product specification overrides them.

Chemical Composition

ASME SA738 Grade B / ASME SA738 GR.B uses the Grade B column. Carbon is tighter than Grade A. Manganese is a range, not only a maximum.

Heat Analysis and Product Analysis — ASME SA738 Grade B (typical Table 1 limits)

Element Heat Analysis (%) Product Analysis (%)
Carbon (C), max 0.20 Per Table 1 of the named edition
Manganese (Mn) 0.90 – 1.50 0.84 – 1.62
Manganese (Mn), >65 mm 0.90 – 1.60 Per Table 1 of the named edition
Phosphorus (P), max Per Table 1 of the named edition Per Table 1 of the named edition
Sulfur (S), max Per Table 1 of the named edition Per Table 1 of the named edition
Silicon, copper, nickel, chromium, molybdenum, vanadium, niobium Per Table 1 of the named edition Per Table 1 of the named edition

Grade A carbon heat is 0.24% max. Grade D carbon heat is 0.10% max. Do not ship Grade A or Grade C as Grade B. Vacuum carbon-deoxidized steel under S17 may replace part of the table when specified. Containment inquiries often add residual and cleanliness limits beyond Table 1. Write those on the order.

SHH STEEL reports heat analysis on every certificate and product analysis when SA-20 requires it. If a Houston, Rotterdam or Jebel Ali specification tightens phosphorus or sulfur, write that on the order.

Mechanical Properties

Grade B is the 85 ksi tensile class.

Tensile Requirements — ASME SA738 Grade B (typical Table 2, ≤50 mm)

Property Requirement
Yield strength, min 415 MPa (60 ksi)
Tensile strength 585 – 705 MPa (85 – 102 ksi)
Elongation in 50 mm, min Per Table 2 of the named edition
Density 7.85 g/cm³
Hardness Not a default substitute for tensile

Tensile columns can change with thickness in Table 2. Confirm the ordered thickness against the named edition. Grade A is 515–655 MPa tensile. Grade C is 550–690 MPa tensile. Grade E is 620–760 MPa tensile. Do not stamp Grade A as Grade B because a coupon came in high.

Density is 7.85 g/cm³. Notch toughness is not optional on most Grade B export orders. Containment and other high-integrity shells write temperature, energy, location and orientation in detail. Simulated PWHT is common because QT plate will see a shop heat cycle after welding.

Material Comparison

Grade Route Strength idea Swap?
SA738 Grade A Heat-treated C-Mn-Si 310 / 515–655, QT only >65 mm No
SA738 Gr.B QT C-Mn-Si 415 / 585–705, QT all t This page
SA738 Grade C QT C-Mn-Si 80 ksi class No
SA738 Grade D / E QT C-Mn-Si 85 / 90 ksi class, thinner cap No
SA516 Gr.70 C-Mn-Si vessel 260 / 485–620 No
SA537 Cl.2 QT carbon Different book No
SA737 Grade C Normalized HSLA 415 / 550–690 No
ASME SA612 High-strength C-Mn-Si Different book No

SA203 Gr.B, SA225 Gr.D and SA455 steel plate are also vessel plates. None of them is ASME SA738 GR.B.

Heat-Treated C-Mn-Si Vessel Service

ASME SA738 Grade B / ASME SA738 GR.B is selected when the vessel wants quenched-and-tempered C-Mn-Si at the 85 ksi tensile class. Typical equipment is high-integrity welded shells, process vessels and reactor containment work written to SA-738 Grade B. Allowable stress comes from ASME Section II Part D after the Code lists this Grade. Project specifications for containment often add toughness, PWHT simulation and NDE beyond the product specification. Those extras belong on the purchase order.

SHH STEEL supplies this plate to fabricators in the United States, Europe, the Middle East and Southeast Asia. It is not nickel low-temp plate like SA203 Gr.D or SA203 Gr.E. It is not QT Ni-Cr-Mo like SA543. It is not SA302 Gr.B. Stainless inquiries belong on ASME SA240 or ASTM A240.

Do not treat Grade B as normalize-only Grade A with a higher coupon. Grade B is QT at every thickness.

Weldability

SA738 Gr.B is killed C-Mn-Si at the 85 ksi class after quench and temper. Welding is Code welding.

Qualify procedures to ASME Section IX. Use consumables written for 585–705 MPa tensile QT carbon, not a SA516 Gr.70 procedure copied across, and not a SA543 Ni-Cr-Mo procedure. Hydrogen control, preheat and PWHT follow the qualified procedure and the vessel specification. Containment WPS packages usually name a PWHT cycle. Plan coupons for that cycle.

Do not copy a SA387 Gr.12 Cl.2 procedure onto SA738 Grade B. The fabricator owns the WPS. SHH STEEL can share mill heat data for that review, including packages prepared for US, EU or Middle East inspectors.

Heat Treatment

Grade B plates in all thicknesses shall be quenched and tempered. When plates are tempered, the minimum tempering temperature is 595 °C (1100 °F). Print austenitizing and tempering temperatures on the certificate when the mill record carries them.

Do not apply the Grade A rule (QT only above 65 mm) to Grade B. Do not ship Grade B as normalized carbon and call it heat-treated.

If the vessel will see PWHT, test coupons shall follow a simulated cycle when the order names it. Special heat treatment, extra simulation or third-party hold points add time. Plan about two months when those extras are on the order.

Delivery Condition

Usual delivery from SHH STEEL is quenched-and-tempered ASME SA738 Grade B / ASME SA738 GR.B plate.

The certificate lists ASME SA738 Grade B and, when dual certified, ASTM A738 Grade B; heat number; heat analysis; product analysis when ordered; tensile results to the Grade B table; QT statement; impact when ordered. Certificates may be EN 10204 3.1 or EN 10204 3.2.

Surface is mill scale unless the order names shot blast, paint or machine allowance. Cutting, beveling and nest sizes belong on the purchase order.

Dimensions

Usual supply range from SHH STEEL for SA738 Gr.B heat-treated vessel plate:

  • Thickness: commonly 8 mm – 100 mm. Current practice normally limits Grade B to about 100 mm
  • Width: 1500 mm – 4000 mm
  • Length: 3000 mm – 12000 mm
  • Cut-to-length shells, heads and nest sizes inside those limits

Structural sizes belong on EN 10025-2 or JIS G3106. Weathering plate belongs on EN 10025-5 or Corten A/B. Fine-grain structural belongs on EN 10025-3 or EN 10025-4. QT structural belongs on EN 10025-6.

Tolerances

Dimensional limits follow ASME SA-20. Thickness, width, length, flatness and camber are vessel-plate tolerances, not structural-plate tolerances from ASTM A36/A36M. UT to A435 / A577 / A578 is commonly added on containment plate. Write the UT level on the order.

Repair welding of surface defects follows SA-20 rules unless the order forbids repair.

Supplementary Requirements

Most export ASME SA738 Grade B / ASME SA738 GR.B orders add extras. SHH STEEL does not assume them.

Charpy details. Temperature, energy, location and orientation. Containment packages often name a lower temperature than ordinary vessel plate.

Simulated PWHT. Same-heat coupons follow the vessel cycle.

NDE. UT to A435 / A577 / A578.

Vacuum carbon deoxidation (S17). When specified.

Through-thickness / Z-direction testing. When the drawing names it.

Third-party. EN 10204 3.2, with inspectors arranged for US, European or Middle East documentation packages.

Equivalent Material Grades

These names are project-comparison grades. They are not automatic substitutes.

Designation Standard / region Notes
ASME SA738 Grade B / ASME SA738 GR.B ASME SA-738/SA-738M Code name on this page
ASTM A738 Grade B ASTM A738/A738M Companion US product spec
SA738 Grade A / C / D / E SA-738 Other strength classes
SA537 Cl.2 SA-537 Related QT carbon
P460NH / P460NL related EN 10028 European comparison only
SPV450 / SPV490 related JIS G3115 Japanese vessel comparison
Q420R / Q460R related GB/T 713 Chinese vessel comparison
SA516 Gr.70 SA-516 Related carbon vessel, different book
ASTM A516 A516 family Related carbon vessel family

DIN 17100, ASME SA515 and ASTM A285 are not SA738 Grade B.

Applications

Industry Typical components
Heat-treated high-integrity vessels ASME SA738 Grade B shells and ASME SA738 GR.B heads
Reactor containment / SA738 Gr.B equipment SA738 Gr.B courses
Dual-certified export SA738 / A738 Grade B plate from SHH STEEL
Fabrication SA738 Gr.B cut to nest sizes

Ship plate inquiries belong on shipbuilding steel plates or BV Rules. Weathering inquiries belong on weathering steel plates. Stainless inquiries belong on stainless steel products, JIS G4305 or AISI stainless.

Other vessel comparisons: SA203 Gr.A, SA302 Gr.C, A516 Grade 70, SA533 Type C Cl.1, SA517 Gr.P.

Global Delivery & Markets

SHH STEEL is a global steel mill sourcing partner with mill partnerships in China. We supply ASTM, ASME, EN and JIS steel to the USA, Europe, Middle East and Southeast Asia. Origin is mill-direct, China origin. We do not treat SA738 Grade B as an Asia-only stock item. Inquiry packages are written for fabricators and EPC buyers in Houston, Rotterdam, Antwerp, Jebel Ali, Dammam, Singapore and surrounding ports.

Typical trade terms:

  • FOB Shanghai
  • CIF Houston
  • CIF Rotterdam
  • CIF Jebel Ali
  • Other CIF / CFR ports on request (Los Angeles, New York, Hamburg, Genoa, Jeddah, Mundra, Ho Chi Minh)

Typical lead time for ASME SA738 Grade B / ASME SA738 GR.B:

  • Ex-stock / ready plate: about 5–7 days after order confirmation, subject to actual warehouse size and cutting
  • Mill rolling, standard QT: about 45 days
  • Special heat treatment, simulated PWHT, 3.2 hold or extra NDE: about 2 months

Documents travel with the cargo: mill certificate, packing list, commercial invoice, bill of lading, and EN 10204 3.1 or 3.2 as ordered. Third-party inspection can be arranged before loading for US, European or Middle East projects. Packing is seaworthy, with edge protection and marking in English as specified on the order.

If the buyer needs a dual ASTM A738 / ASME SA738 stamp for a Section VIII vessel in the United States, say so on the inquiry. If the buyer needs a PED / 3.2 file for Europe, say so on the inquiry. Do not assume a domestic Chinese certificate format will pass at destination.

Why Choose SHH STEEL

SHH STEEL is a global steel mill sourcing partner and steel manufacturer & exporter (mill-direct, China origin). We supply ASTM / EN / JIS steel to the USA, Europe, the Middle East and Southeast Asia. On ASME SA738 Grade B / ASME SA738 GR.B that means mill pricing, dual SA738/A738 marking, Grade B chemistry reported, recorded quench and temper, tensile results at 415 MPa yield and 585–705 MPa tensile, 3.1 as standard and 3.2 when specified. Trade terms include FOB Shanghai and CIF Houston / Rotterdam / Jebel Ali.

We keep the Grade on the order. Grade B is not Grade A. Grade B is QT at every thickness. SA738 Grade B is not SA516 Grade 70. SA738 Grade B is not SA737 Grade B. SA738 is not SA387 Gr.22 Cl.2. If the drawing names containment extras, we will not ship a bare mill certificate and call it complete.

Company scope: global steel mill sourcing partner – SHH STEEL.

FAQ

What names are used for ASME SA738 Grade B / ASME SA738 GR.B?
Buyers write ASME SA738 Grade B, ASME SA738 GR.B, SA738 Gr.B, SA738GRB, SA-738 Grade B, A738 Grade B and ASTM A738 Gr.B. SHH STEEL prints the wording on the purchase order.
Is ASME SA738 Grade B the same as ASTM A738 Grade B?
Chemistry and tensile limits match. ASME SA-738 is the Code version. ASTM A738 is the product spec. SHH STEEL dual-certifies both names when the vessel must be stamped in the United States or elsewhere.
What is the yield strength of SA738 Gr.B?
415 MPa minimum. Tensile is 585–705 MPa on the usual thickness column. Confirm Table 2 for the ordered thickness.
Must ASME SA738 GR.B be quenched and tempered?
Yes. Grade B is QT in all thicknesses. Grade A is QT only above 65 mm.
Why is SA738 Grade B asked for containment vessels?
Grade B is the 85 ksi QT C-Mn-Si class with toughness that containment specifications can build on. The product specification alone is not a containment certificate. Write the project extras on the order.
Can SHH STEEL ship ASME SA738 Grade B outside Asia?
Yes. SHH STEEL is a global steel mill sourcing partner. We supply this plate to the USA, Europe, the Middle East and Southeast Asia on FOB Shanghai or CIF Houston / Rotterdam / Jebel Ali.
What is the delivery time for SA738 Gr.B?
Ex-stock about 5–7 days. Standard mill QT about 45 days. Special heat treatment, simulated PWHT or 3.2 inspection about 2 months.
Can welding of SA738 Grade B be qualified to ASME Section IX?
Yes. Use a WPS written for this QT C-Mn-Si tensile band. The fabricator owns the procedure.

Conclusion

ASME SA738 Grade B Steel Plate, also searched as ASME SA738 GR.B, is quenched-and-tempered C-Mn-Si plate under ASME SA-738/SA-738M for moderate and lower temperature welded vessels, at 415 MPa yield and 585–705 MPa tensile. Whether the inquiry says ASME SA738 Grade B, ASME SA738 GR.B, SA738 Gr.B or A738 Grade B, SHH STEEL as a global steel mill sourcing partner and steel manufacturer & exporter (mill-direct, China origin) supplies plate with Grade B chemistry, recorded QT delivery, and EN 10204 3.1 or 3.2 certification.

SHH STEEL supplies ASME SA738 Grade B / SA738 Gr.B Heat-Treated Vessel Plate to the USA, Europe, the Middle East and Southeast Asia for ASME Section VIII work that actually names this Grade. FOB Shanghai / CIF Houston / Rotterdam / Jebel Ali.

Contact SHH STEEL for mill rolling, stock inquiry, dual SA738/A738 marking, impact testing, 3.2 inspection or a quotation.

ASME SA738 Grade B Steel Plate, ASME SA738 GR.B, SA738 Gr.B, SA738GRB, SA-738 Grade B, A738 Grade B, heat-treated vessel plate, containment vessel plate, global steel mill sourcing partner SHH STEEL

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X