NB/T 47002.1 321 S32168 + 15CrMoR Stainless Steel Clad Plate

NB/T 47002.1 321 S32168 + 15CrMoR stainless steel clad plate bonds titanium-stabilized 06Cr18Ni11Ti to 1Cr-0.5Mo 15CrMoR for GB/T 150 vessels running hot, including hydrogen service. Both layers tolerate the required PWHT. SHH STEEL produces it in China by explosion welding, with 100 % UT and N+T base delivery.
Keywords
NB/T 47002.1 S32168 + 15CrMoR, 321 + 15CrMoR clad plate, Cr-Mo stainless clad plate, 15CrMoR clad plate, hydrogen service clad plate
Equivalent Grades:
GB/T 8165, ASTM A264 / ASME SA-264; S32168 = 321; 15CrMoR ≈ SA387 Gr.12 Cl.2 / 13CrMo4-5 (approx.)
Share:
General Description
Material Specification
Base and Cladding Materials
Sizes and Classes
Chemical Composition
Mechanical Properties
Heat Treatment
Bond Inspection
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is NB/T 47002.1 321 S32168 + 15CrMoR stainless steel clad plate?

NB/T 47002.1 321 S32168 + 15CrMoR stainless steel clad plate is a pressure vessel clad plate in which 06Cr18Ni11Ti (S32168) stainless steel is bonded by explosion welding or roll bonding to 15CrMoR chromium-molybdenum pressure vessel steel. It is ordered to NB/T 47002.1-2019, the energy industry standard that GB/T 150 points to for stainless steel-steel clad plate in pressure vessels. The 15CrMoR carries the design pressure; the S32168 layer is the corrosion barrier.

It is written S32168 + 15CrMoR, or 1Cr18Ni9Ti + 15CrMoR on older drawings. 15CrMoR is listed by name in NB/T 47002.1 Table 2 and is the 1Cr-0.5Mo pressure vessel steel for elevated temperature and hydrogen-bearing service. A titanium-stabilized cladding is the natural partner, because these vessels are always post-weld heat treated and often run in the sensitizing range.

Typical users are refinery hydrotreaters, reformers and coal chemical units, where the Cr-Mo shell resists high-temperature hydrogen attack and the stainless layer resists sulfide and polythionic acid corrosion.

SHH STEEL can produce S32168 + 15CrMoR clad plate to NB/T 47002.1, marked with its class code (B1 or B2 for explosion bonded plate, R1 or R2 for roll bonded plate) and certified with the full test set. Typical claddings are 2 to 16 mm on bases from 6 mm upward.

NB/T 47002.1-2019 requirements for S32168 + 15CrMoR

NB/T 47002.1-2019 covers clad plate with a stainless steel cladding and a carbon steel, low-alloy steel or stainless steel base, made by explosion welding or roll bonding, for pressure vessels with a total thickness of 8 mm or more. It replaced NB/T 47002.1-2009, which itself replaced JB 4733-1996, and it took effect on 1 May 2020.

What changed in the 2019 edition

  • Roll bonded plate was added, with its own limits on total thickness, base-to-cladding thickness ratio, tolerances and class codes.
  • Requirements were added for stress relief heat treatment of clad plate and the equipment used.
  • Duplex stainless claddings now need a phase ratio check in the delivered condition.
  • A side bend test was added, and the inner bend test was extended from class 1 to classes 1 and 2.
  • Visual testing to NB/T 47013.7 was added, and intergranular corrosion testing of the cladding to GB/T 4334 can be specified.

Place in the GB/T 150 system

GB/T 150.2 requires stainless steel-steel clad plate for pressure vessels to meet NB/T 47002.1, requires the design documents to state the clad plate class, and limits the unbonded ratio. If a designer chooses another clad plate standard instead, the interface shear strength must still be at least 210 MPa. The service temperature range of the clad plate must satisfy the limits for both the base and the cladding.

What the order must state

Item Example for this product
Standard number NB/T 47002.1-2019
Product name Stainless steel-steel clad plate
Cladding and base grades S32168 + 15CrMoR
Manufacturing method and class Explosion welded class 1 (B1), or as required
Delivery condition Normalized and tempered base, per GB/T 150
Dimensions Cladding + base thickness × width × length, or diameter
Weight Theoretical or actual
Additional requirements For example intergranular corrosion test, cladding surface finish

S32168 cladding and 15CrMoR base

NB/T 47002.1 Table 2 lists the cladding and base standards. Claddings come from GB/T 24511 (pressure equipment stainless plate, now continued as GB/T 713.7), with examples S11306, S11348, S30408, S30403, S32168, S31603, S31703, S39042, S22053 and S25073. Bases come from GB/T 713 (Q245R, Q345R, 15CrMoR), GB/T 3531 (16MnDR, 09MnNiDR), the forging standards NB/T 47008, 47009 and 47010, or GB/T 24511 for stainless bases. Other grades from the listed standards may also be used.

Three rules in clause 7.1 matter in practice. Forged bases must be class III or IV forgings. A base whose specified minimum tensile strength exceeds 540 MPa needs a technical review before use. Materials from standards outside Table 2 are allowed by agreement only if their requirements, including P and S limits and impact test temperature and energy, are no lower than those of the nearest Table 2 grade.

Why 06Cr18Ni11Ti (S32168) is used

S32168 (06Cr18Ni11Ti) carries titanium at least five times its carbon content, so carbon is bound as titanium carbide and chromium stays in solution at grain boundaries. On a Cr-Mo vessel this matters twice: the shell is post-weld heat treated for hours at 650 to 700 °C, and in service the cladding may sit in the sensitizing range for years.

In refinery hydrotreating units the cladding also has to resist polythionic acid stress corrosion cracking during shutdowns, when sulfide scales react with air and moisture. Stabilized grades such as S32168 and 347 types are the usual answer, often combined with shutdown neutralization procedures.

15CrMoR base steel

GB/T 713 15CrMoR is the 1Cr-0.5Mo pressure vessel plate of GB/T 713.2-2023 for elevated-temperature, hydrogen-bearing service. It is delivered normalized and tempered, with tempering not below 650 °C, and has 295 MPa minimum yield and 450 to 590 MPa tensile strength up to 60 mm, with 47 J at 20 °C as the usual impact requirement. It is listed by name in NB/T 47002.1 Table 2 as a base material.

Design notes

The base sets the temperature limit and the hydrogen resistance; check the Nelson-curve data and GB/T 150 temperature limits for 15CrMoR. The cladding protects against corrosion; S32168 resists sensitization during the long PWHT that Cr-Mo vessels require.

Specify the PWHT temperature and hold so the clad plate maker can test simulated coupons. 15CrMoR is tempered at 650 °C or above, so PWHT below the tempering temperature does not change its delivery condition.

Dimensions, class codes and marking

Item NB/T 47002.1-2019 rule
Cladding thickness Preferably 2 – 16 mm
Base thickness 6 mm minimum
Base / cladding thickness ratio Not less than 2 for roll bonding; not less than 3 for explosion welding
Roll bonded plate Total thickness generally not over 100 mm
Explosion welded plate Area generally not over 25 m²
Larger sizes By agreement
Form Single- or double-sided; rectangular, square or round
Weight Theoretical weight allowed; stainless densities in Annex A

Each plate carries a class and a code that shows the manufacturing method: B for explosion welded plate and R for roll bonded plate, followed by the class number, for example B1, B2 or R2. Each class sets the allowable unbonded ratio and the size of individual unbonded areas. A double-sided plate states the class of each face separately.

Marking examples

The standard’s own examples show the format: (S32168+Q345R)-(3+16)×2500×8000-R2-NB/T 47002.1—2019 for 3 mm S32168 roll bonded to 16 mm Q345R, class 2; and (S30408+16MnⅢ)-(8+150)×D4000-B1-NB/T 47002.1—2019 for an explosion welded tube sheet on a class III 16Mn forging.

For this product, 3 mm S32168 explosion welded to 30 mm 15CrMoR, 2000 × 6000 mm, class 1, is marked (S32168+15CrMoR)-(3+30)×2000×6000-B1-NB/T 47002.1—2019.

Chemical composition of S32168 cladding and 15CrMoR base

Under NB/T 47002.1 the cladding is normally certified to GB/T 24511 / GB/T 713.7, the pressure equipment stainless standards, which keep the alloy ranges of the general grade and tighten some residual limits. The table shows the GB/T 4237 limits of S32168 for reference; the certificate reports the limits of the standard actually ordered.

06Cr18Ni11Ti (S32168) cladding

Element S32168 heat analysis, % (GB/T 4237) Permitted deviation, % Product analysis limit, %
C ≤ 0.08 +0.01 ≤ 0.09
Si ≤ 0.75 +0.05 ≤ 0.80
Mn ≤ 2.00 +0.04 ≤ 2.04
P ≤ 0.045 +0.010 ≤ 0.055
S ≤ 0.030 +0.005 ≤ 0.035
Cr 17.00 – 19.00 ±0.20 16.80 – 19.20
Ni 9.00 – 12.00 −0.10 at min / +0.15 at max 8.90 – 12.15
N ≤ 0.10 +0.01 ≤ 0.11
Ti ≥ 5 × C — —

15CrMoR base steel (GB/T 713.2)

Element 15CrMoR heat analysis, % 15CrMoR product analysis, %
C 0.12 – 0.18 0.10 – 0.20
Si 0.15 – 0.40 0.13 – 0.45
Mn 0.40 – 0.70 0.35 – 0.75
P ≤ 0.025 ≤ 0.030
S ≤ 0.010 ≤ 0.015
Cr 0.80 – 1.20 0.75 – 1.25
Mo 0.45 – 0.60 0.43 – 0.63
Cu / Ni ≤ 0.30 each ≤ 0.34 each

15CrMoR limits sulfur to 0.010 % and phosphorus to 0.025 %. Because it is tempered at 650 °C or above, a clad plate stress relief below the tempering temperature does not change its delivery condition, which NB/T 47002.1 notes explicitly.

Mechanical properties and bond tests

NB/T 47002.1 tests the clad plate as a composite. It defines the yield strength used for the composite as any one of ReH, ReL, Rp0.2, Rt0.5 or Rr0.2, taken from each layer’s own material standard, so that the base and cladding values can be combined in the calculation of the clad plate’s yield strength.

Test Purpose
Tensile test Composite strength and elongation against the calculated and base requirements
Shear test Interface bond strength; 210 MPa is the GB/T 150.2 benchmark for stainless clad plate
Inner bend Cladding in compression; required for classes 1 and 2 since 2019
Outer bend Cladding in tension; checks the cladding and the interface
Side bend Added in 2019; bends across the interface
Impact test On the base, as the base standard and GB/T 150 require

Worked example for 3 + 30 mm S32168 + 15CrMoR: the base over 6 to 60 mm has 295 MPa minimum yield and 450 MPa minimum tensile, and S32168 has 205 and 515 MPa. The thickness-weighted average, the method used in Chinese clad plate standards, gives (3 × 205 + 30 × 295) / 33 = 287 MPa for yield and (3 × 515 + 30 × 450) / 33 = 456 MPa for tensile. Designers who do not count the cladding simply use the base values for the base thickness.

15CrMoR base strength by thickness

15CrMoR thickness, mm Yield strength min, MPa Tensile strength, MPa
6 – 60 295 450 – 590
> 60 – 100 275 450 – 590
> 100 – 200 255 440 – 580

S32168 cladding strength

Property 06Cr18Ni11Ti (S32168)
Proof strength Rp0.2 ≥ 205 MPa
Tensile strength Rm ≥ 515 MPa
Elongation A ≥ 40 %
Hardness ≤ 217 HBW, ≤ 95 HRB, ≤ 220 HV

Test methods for clad plate mechanical and bend properties follow GB/T 6396; tensile tests follow GB/T 228.1 and impact tests GB/T 229.

Delivery condition and stress relief

Clause 7.2 requires clad plate to be delivered flattened and sheared or cut, with the base in the hot-rolled or heat-treated condition that GB/T 150 or JB 4732 requires for that steel. Other conditions are possible by agreement in the contract. On request the cladding surface can be blasted, polished or pickled.

Stress relief of clad plate should follow GB/T 30583. The standard notes that a stress relief below the base’s tempering temperature is generally considered not to change the base’s delivery condition.

S32168 + 15CrMoR is delivered with the base normalized and tempered. Where bonding precedes the base heat treatment, the clad plate is normalized and tempered as a whole; S32168 tolerates the cycle because titanium ties up carbon, and the cladding is pickled again afterwards.

Impact tests on the base, commonly 47 J at 20 °C, and simulated PWHT coupons are reported on the certificate.

Ultrasonic testing and repair of unbonded areas

Every clad plate is ultrasonically tested with 100 % scanning to NB/T 47013.3, and the bond must meet the class limits in Table 3: the length of any single unbonded indication, the area of any single unbonded zone, and the total unbonded ratio. Surfaces are checked visually to NB/T 47013.7.

Unbonded areas beyond the Table 3 limits may be repaired. The cladding over the area is removed and ground down to the base, penetrant testing confirms that the unbonded zone is gone, and a certified welder repairs it with a procedure qualified to NB/T 47014. The repair is then checked by UT, which must meet Table 3, and by penetrant testing to NB/T 47013.5-2015 class I. The repair record, with location, area, filler and welding parameters, is attached to the quality certificate.

For tube sheets cut from S32168 + 15CrMoR plate, GB/T 151 asks for explosion clad plate to class B1, so specify B1 for any plate that will be drilled.

Typical thickness combinations of S32168 + 15CrMoR

S32168 + 15CrMoR clad plate is specified by cladding and base thickness, width and length, or diameter for discs. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
3 + 20 23 Hot separators
3 + 25 28 Drums
3 + 30 33 Reactors
4 + 36 40 Hydrotreater shells
4 + 44 48 Thick shells
5 + 56 61 Heavy shells
6 + 70 and over 76 and over Heavy reactors and tube sheets
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Welding S32168 + 15CrMoR clad plate

Pressure vessel seams in S32168 + 15CrMoR are welded base first, then the cladding is restored. Procedures are qualified to NB/T 47014 and welding follows NB/T 47015.

  1. Prepare the bevel and strip the cladding back from the root as the procedure requires.
  2. Weld the 15CrMoR with low-hydrogen filler matching the base, for example E5515-B2 / ER55-B2 type 1Cr-0.5Mo filler, with preheat and PWHT as the qualified procedure requires.
  3. Back-gouge from the clad side to sound base weld metal.
  4. Lay the transition layer with an E309L / ER309L type filler.
  5. Finish with E347 / ER347 filler, because titanium does not transfer across the arc and niobium gives the weld the stabilization.
  6. Pickle and passivate the weld zone.

Weld the 15CrMoR with matching Cr-Mo low-hydrogen filler and preheat, commonly around 150 °C or as the qualified procedure requires, then apply the 309L transition and 347 cap to the cladding. PWHT follows the Cr-Mo requirements in GB/T 150 and NB/T 47015.

Applications of S32168 + 15CrMoR clad plate (NB/T 47002.1)

S32168 + 15CrMoR NB/T 47002.1 clad plate is used in hot, hydrogen-bearing GB/T 150 vessels.

  • Refinery hydrotreater reactors and hot separators.
  • Catalytic reformer vessels.
  • Hydrocracker drums in moderate temperature zones.
  • Coal chemical shift converters.
  • Hot high-pressure heat exchanger shells.
  • Petrochemical reactors with sulfur-bearing feed.

Heavier Cr-Mo bases

For higher temperature or hydrogen partial pressure, 14Cr1MoR or 12Cr2Mo1R bases are used with stainless overlay or clad plate; these are agreed case by case with the vessel designer.

Material certificates and quality documents

Clause 7.1.5 requires the original mill certificates of the cladding and base, complete and stamped by the mill’s inspection department. If the clad plate maker holds only copies, they must carry the stockist’s inspection stamp and a signature, and the clad plate maker is responsible for their authenticity and consistency. This is why we buy cladding and base directly from mills.

Document or test Content
Base and cladding mill certificates Original, or stamped and signed copies
Clad plate certificate Tests of the clad plate, UT results per plate, class code
Repair record Location, area, filler and parameters of any repair
Packaging and marking GB/T 247
Optional Intergranular corrosion per GB/T 4334, third-party inspection, EN 10204 3.1 or 3.2

Equivalent standards and grades

NB/T 47002.1 is the pressure vessel standard; GB/T 8165 is the general stainless clad plate standard. The same pairing can be ordered to either, but a GB/T 150 vessel should cite NB/T 47002.1.

Standard Use Bond shear Classes
NB/T 47002.1-2019 Pressure vessels under GB/T 150 210 MPa benchmark (GB/T 150.2) B1/B2, R1/R2
GB/T 8165-2025 General stainless clad plate and strip 250 MPa (grades 1–2), 210 MPa (grade 3) B/R/BR 1–3
ASTM A264 / ASME SA-264 ASME vessels 140 MPa when specified Class 1/3/5
JIS G3601 JIS vessels 200 N/mm² Class 1/2
Layer GB ASTM / ASME UNS EN JIS
Cladding 06Cr18Ni11Ti (S32168) A240 / SA-240 321 S32100 1.4541 SUS321
Base 15CrMoR (GB/T 713.2) SA387 Gr.12 Cl.2 (approx.) K11757 13CrMo4-5 (approx.) SCMV2 (approx.)

For ASME Code work the nearest product is SA387 Gr.12 Cl.2 + 321 to ASTM A264 / ASME SA-264; for general Chinese supply the same pairing is ordered to GB/T 8165. Equivalence is approximate, so check strength, tests and class against the design code before substituting.

Why order NB/T 47002.1 S32168 + 15CrMoR from SHH STEEL

SHH STEEL is a clad plate manufacturer in China that supplies NB/T 47002.1 plate to vessel shops working under TSG 21 and GB/T 150. For S32168 + 15CrMoR we coordinate the N+T and PWHT sequence and supply simulated PWHT coupons.

  • We agree the class code with you before production, since it fixes the UT acceptance and the tests.
  • Mill certificates of cladding and base are originals from the mills, as clause 7.1.5 asks.
  • Every plate is UT scanned 100 % and marked in the NB/T format.
  • Plates can be cut to head blanks and tube sheet discs.

FAQ

Why pair 321 cladding with 15CrMoR?
Cr-Mo vessels are always PWHT'd and often run in the sensitizing range; titanium-stabilized S32168 keeps its intergranular corrosion resistance.
Is 15CrMoR listed in NB/T 47002.1?
Yes, 15CrMoR is one of the GB/T 713 base examples in Table 2.
What is the composite strength of 3 + 30 mm S32168 + 15CrMoR?
By the thickness-weighted method, about 287 MPa yield and 456 MPa tensile minimum.
Which filler welds the 15CrMoR base?
Matching 1Cr-0.5Mo low-hydrogen filler, such as E5515-B2 / ER55-B2 type, with preheat and PWHT.
What is the difference between NB/T 47002.1 and GB/T 8165?
NB/T 47002.1 is the pressure vessel standard referenced by GB/T 150, with classes B1/B2 and R1/R2 and a total thickness of 8 mm or more. GB/T 8165 is the general stainless clad plate standard with grades 1 to 3 and B, R and BR codes.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
NB/T 47002.1-2019, S32168 + 15CrMoR, cladding and base thickness, class code (for example B1), size, quantity, delivery condition, extra tests and certificate type.

Request a quotation for NB/T 47002.1 321 S32168 + 15CrMoR Stainless Steel Clad Plate

NB/T 47002.1 321 S32168 + 15CrMoR stainless steel clad plate combines titanium-stabilized cladding with 1Cr-0.5Mo 15CrMoR for hot, hydrogen-bearing GB/T 150 vessels. It is classed B1/B2, 100 % UT tested and supplied with the base normalized and tempered.

Send the thickness pair, class code, plate size and quantity to SHH STEEL, or see related plates under GB/T 8165 and ASTM A264. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X