NB/T 47002.1 316L S31603 + Q370R Stainless Steel Clad Plate
What is NB/T 47002.1 316L S31603 + Q370R stainless steel clad plate?
NB/T 47002.1 316L S31603 + Q370R stainless steel clad plate is a pressure vessel clad plate in which 022Cr17Ni12Mo2 (S31603) stainless steel is bonded by explosion welding or roll bonding to Q370R pressure vessel steel. It is ordered to NB/T 47002.1-2019, the energy industry standard that GB/T 150 points to for stainless steel-steel clad plate in pressure vessels. The Q370R carries the design pressure; the S31603 layer is the corrosion barrier.
It is written S31603 + Q370R, or 316L + 15MnNbR on older drawings. Q370R is a GB/T 713 grade and so falls within the base standards of NB/T 47002.1 Table 2, although the table’s examples name Q245R, Q345R and 15CrMoR. It is a niobium-microalloyed, normalized fine-grain steel with 370 MPa minimum yield.
The pairing is used when a large 316L clad vessel would need a very thick Q345R shell. Moving to Q370R reduces thickness and weight, and with it bonding, rolling, welding and transport costs.
SHH STEEL can produce S31603 + Q370R clad plate to NB/T 47002.1, marked with its class code (B1 or B2 for explosion bonded plate, R1 or R2 for roll bonded plate) and certified with the full test set. Typical claddings are 2 to 16 mm on bases from 6 mm upward.
NB/T 47002.1-2019 requirements for S31603 + Q370R
NB/T 47002.1-2019 covers clad plate with a stainless steel cladding and a carbon steel, low-alloy steel or stainless steel base, made by explosion welding or roll bonding, for pressure vessels with a total thickness of 8 mm or more. It replaced NB/T 47002.1-2009, which itself replaced JB 4733-1996, and it took effect on 1 May 2020.
What changed in the 2019 edition
- Roll bonded plate was added, with its own limits on total thickness, base-to-cladding thickness ratio, tolerances and class codes.
- Requirements were added for stress relief heat treatment of clad plate and the equipment used.
- Duplex stainless claddings now need a phase ratio check in the delivered condition.
- A side bend test was added, and the inner bend test was extended from class 1 to classes 1 and 2.
- Visual testing to NB/T 47013.7 was added, and intergranular corrosion testing of the cladding to GB/T 4334 can be specified.
Place in the GB/T 150 system
GB/T 150.2 requires stainless steel-steel clad plate for pressure vessels to meet NB/T 47002.1, requires the design documents to state the clad plate class, and limits the unbonded ratio. If a designer chooses another clad plate standard instead, the interface shear strength must still be at least 210 MPa. The service temperature range of the clad plate must satisfy the limits for both the base and the cladding.
What the order must state
| Item | Example for this product |
|---|---|
| Standard number | NB/T 47002.1-2019 |
| Product name | Stainless steel-steel clad plate |
| Cladding and base grades | S31603 + Q370R |
| Manufacturing method and class | Explosion welded class 1 (B1), or as required |
| Delivery condition | Normalized or normalized and tempered base, per GB/T 150 |
| Dimensions | Cladding + base thickness × width × length, or diameter |
| Weight | Theoretical or actual |
| Additional requirements | For example intergranular corrosion test, cladding surface finish |
S31603 cladding and Q370R base
NB/T 47002.1 Table 2 lists the cladding and base standards. Claddings come from GB/T 24511 (pressure equipment stainless plate, now continued as GB/T 713.7), with examples S11306, S11348, S30408, S30403, S32168, S31603, S31703, S39042, S22053 and S25073. Bases come from GB/T 713 (Q245R, Q345R, 15CrMoR), GB/T 3531 (16MnDR, 09MnNiDR), the forging standards NB/T 47008, 47009 and 47010, or GB/T 24511 for stainless bases. Other grades from the listed standards may also be used.
Three rules in clause 7.1 matter in practice. Forged bases must be class III or IV forgings. A base whose specified minimum tensile strength exceeds 540 MPa needs a technical review before use. Materials from standards outside Table 2 are allowed by agreement only if their requirements, including P and S limits and impact test temperature and energy, are no lower than those of the nearest Table 2 grade.
Why 022Cr17Ni12Mo2 (S31603) is used
S31603 is the standard molybdenum-bearing low-carbon cladding. On a large Q370R vessel the cladding is usually 3 to 4 mm thick, and because the vessel is large, the cladding is a big share of the material cost; keeping it to the corrosion allowance actually needed is worthwhile.
S31603 tolerates the normalizing that a Q370R base may need after bonding, because its low carbon prevents sensitization. It resists chlorides and dilute acids far better than 304, which is why it is chosen for large chemical and coal chemical reactors.
Q370R base steel
GB/T 713 Q370R is the niobium-microalloyed, fine-grain pressure vessel plate of GB/T 713.2-2023, known on older drawings as 15MnNbR. It is delivered normalized or normalized and tempered, has 370 MPa minimum yield up to 16 mm and is commonly impact tested at −20 °C. In a clad vessel it is chosen when Q345R would make the shell too thick, typically for larger, higher-pressure reactors and columns.
Design notes
Q370R’s specified minimum tensile strength is 530 MPa, below the 540 MPa threshold above which NB/T 47002.1 requires a technical review of the base. Its toughness depends on the normalized fine-grain structure, so the clad plate maker must preserve or restore that condition.
Agree any stress relief temperature with the maker; it should stay below the tempering temperature if the base is supplied normalized and tempered.
Dimensions, class codes and marking
| Item | NB/T 47002.1-2019 rule |
|---|---|
| Cladding thickness | Preferably 2 – 16 mm |
| Base thickness | 6 mm minimum |
| Base / cladding thickness ratio | Not less than 2 for roll bonding; not less than 3 for explosion welding |
| Roll bonded plate | Total thickness generally not over 100 mm |
| Explosion welded plate | Area generally not over 25 m² |
| Larger sizes | By agreement |
| Form | Single- or double-sided; rectangular, square or round |
| Weight | Theoretical weight allowed; stainless densities in Annex A |
Each plate carries a class and a code that shows the manufacturing method: B for explosion welded plate and R for roll bonded plate, followed by the class number, for example B1, B2 or R2. Each class sets the allowable unbonded ratio and the size of individual unbonded areas. A double-sided plate states the class of each face separately.
Marking examples
The standard’s own examples show the format: (S32168+Q345R)-(3+16)×2500×8000-R2-NB/T 47002.1—2019 for 3 mm S32168 roll bonded to 16 mm Q345R, class 2; and (S30408+16MnⅢ)-(8+150)×D4000-B1-NB/T 47002.1—2019 for an explosion welded tube sheet on a class III 16Mn forging.
For this product, 4 mm S31603 explosion welded to 30 mm Q370R, 2200 × 7000 mm, class 2, is marked (S31603+Q370R)-(4+30)×2200×7000-B2-NB/T 47002.1—2019.
Chemical composition of S31603 cladding and Q370R base
Under NB/T 47002.1 the cladding is normally certified to GB/T 24511 / GB/T 713.7, the pressure equipment stainless standards, which keep the alloy ranges of the general grade and tighten some residual limits. The table shows the GB/T 4237 limits of S31603 for reference; the certificate reports the limits of the standard actually ordered.
022Cr17Ni12Mo2 (S31603) cladding
| Element | S31603 heat analysis, % (GB/T 4237) | Permitted deviation, % | Product analysis limit, % |
|---|---|---|---|
| C | ≤ 0.030 | +0.005 | ≤ 0.035 |
| Si | ≤ 0.75 | +0.05 | ≤ 0.80 |
| Mn | ≤ 2.00 | +0.04 | ≤ 2.04 |
| P | ≤ 0.045 | +0.010 | ≤ 0.055 |
| S | ≤ 0.030 | +0.005 | ≤ 0.035 |
| Cr | 16.00 – 18.00 | ±0.20 | 15.80 – 18.20 |
| Ni | 10.00 – 14.00 | −0.10 at min / +0.15 at max | 9.90 – 14.15 |
| Mo | 2.00 – 3.00 | ±0.10 | 1.90 – 3.10 |
| N | ≤ 0.10 | +0.01 | ≤ 0.11 |
Q370R base steel (GB/T 713.2)
| Element | Q370R heat analysis, % | Q370R product analysis, % |
|---|---|---|
| C | ≤ 0.18 | ≤ 0.20 |
| Si | ≤ 0.55 | ≤ 0.60 |
| Mn | 1.20 – 1.70 | 1.15 – 1.80 |
| P | ≤ 0.020 | ≤ 0.025 |
| S | ≤ 0.010 | ≤ 0.015 |
| Nb | 0.015 – 0.050 | 0.010 – 0.055 |
| V | ≤ 0.050 | ≤ 0.055 |
| Ti | ≤ 0.030 | ≤ 0.035 |
| Cr / Ni / Cu | ≤ 0.30 each | ≤ 0.34 each |
| Mo | ≤ 0.08 | ≤ 0.09 |
| Cu + Ni + Cr + Mo | ≤ 0.70 | ≤ 0.75 |
Q370R limits phosphorus to 0.020 % and sulfur to 0.010 %. Its niobium refines the grain, which gives the base its low-temperature toughness; the clad plate supplier must keep the base in the normalized condition through bonding and any stress relief.
Mechanical properties and bond tests
NB/T 47002.1 tests the clad plate as a composite. It defines the yield strength used for the composite as any one of ReH, ReL, Rp0.2, Rt0.5 or Rr0.2, taken from each layer’s own material standard, so that the base and cladding values can be combined in the calculation of the clad plate’s yield strength.
| Test | Purpose |
|---|---|
| Tensile test | Composite strength and elongation against the calculated and base requirements |
| Shear test | Interface bond strength; 210 MPa is the GB/T 150.2 benchmark for stainless clad plate |
| Inner bend | Cladding in compression; required for classes 1 and 2 since 2019 |
| Outer bend | Cladding in tension; checks the cladding and the interface |
| Side bend | Added in 2019; bends across the interface |
| Impact test | On the base, as the base standard and GB/T 150 require |
Worked example for 4 + 30 mm S31603 + Q370R: the base over 16 to 36 mm has 360 MPa minimum yield and 530 MPa minimum tensile, and S31603 has 180 and 485 MPa. The thickness-weighted average, the method used in Chinese clad plate standards, gives (4 × 180 + 30 × 360) / 34 = 339 MPa for yield and (4 × 485 + 30 × 530) / 34 = 525 MPa for tensile. Designers who do not count the cladding simply use the base values for the base thickness.
Q370R base strength by thickness
| Q370R thickness, mm | Yield strength min, MPa | Tensile strength, MPa |
|---|---|---|
| 6 – 16 | 370 | 530 – 630 |
| > 16 – 36 | 360 | 530 – 630 |
| > 36 – 60 | 340 | 520 – 620 |
| > 60 – 100 | 330 | 510 – 610 |
S31603 cladding strength
| Property | 022Cr17Ni12Mo2 (S31603) |
|---|---|
| Proof strength Rp0.2 | ≥ 180 MPa |
| Tensile strength Rm | ≥ 485 MPa |
| Elongation A | ≥ 40 % |
| Hardness | ≤ 217 HBW, ≤ 95 HRB, ≤ 220 HV |
Test methods for clad plate mechanical and bend properties follow GB/T 6396; tensile tests follow GB/T 228.1 and impact tests GB/T 229.
Delivery condition and stress relief
Clause 7.2 requires clad plate to be delivered flattened and sheared or cut, with the base in the hot-rolled or heat-treated condition that GB/T 150 or JB 4732 requires for that steel. Other conditions are possible by agreement in the contract. On request the cladding surface can be blasted, polished or pickled.
Stress relief of clad plate should follow GB/T 30583. The standard notes that a stress relief below the base’s tempering temperature is generally considered not to change the base’s delivery condition.
S31603 + Q370R is delivered with the base in the normalized or normalized and tempered condition GB/T 150 requires. If the bonding sequence would disturb that condition, the clad plate is renormalized; S31603’s low carbon tolerates the cycle without sensitization, although the cladding is then pickled again.
Impact tests on the base, commonly at −20 °C, are made on the clad plate in its final condition.
Ultrasonic testing and repair of unbonded areas
Every clad plate is ultrasonically tested with 100 % scanning to NB/T 47013.3, and the bond must meet the class limits in Table 3: the length of any single unbonded indication, the area of any single unbonded zone, and the total unbonded ratio. Surfaces are checked visually to NB/T 47013.7.
Unbonded areas beyond the Table 3 limits may be repaired. The cladding over the area is removed and ground down to the base, penetrant testing confirms that the unbonded zone is gone, and a certified welder repairs it with a procedure qualified to NB/T 47014. The repair is then checked by UT, which must meet Table 3, and by penetrant testing to NB/T 47013.5-2015 class I. The repair record, with location, area, filler and welding parameters, is attached to the quality certificate.
For tube sheets cut from S31603 + Q370R plate, GB/T 151 asks for explosion clad plate to class B1, so specify B1 for any plate that will be drilled.
Typical thickness combinations of S31603 + Q370R
S31603 + Q370R clad plate is specified by cladding and base thickness, width and length, or diameter for discs. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.
| Cladding + base, mm | Total, mm | Typical use |
|---|---|---|
| 3 + 20 | 23 | Medium shells |
| 3 + 25 | 28 | Reactors |
| 4 + 30 | 34 | Large reactors |
| 4 + 36 | 40 | Columns |
| 4 + 44 | 48 | Thick shells |
| 5 + 50 | 55 | Heavy shells |
| 6 + 60 and over | 66 and over | Very large vessels, explosion welded |
| Dimension | Production range |
|---|---|
| Cladding thickness | 2 mm to 20 mm (thicker by explosion bonding on request) |
| Base steel thickness | 6 mm to 200 mm |
| Total thickness | 8 mm to 220 mm |
| Width | 1000 mm to 3000 mm; wider by explosion bonding with welded cladding |
| Length | 2000 mm to 12000 mm |
| Discs and blanks | Round tube sheet blanks and head blanks cut to drawing |
| Location | China |
Welding S31603 + Q370R clad plate
Pressure vessel seams in S31603 + Q370R are welded base first, then the cladding is restored. Procedures are qualified to NB/T 47014 and welding follows NB/T 47015.
- Prepare the bevel and strip the cladding back from the root as the procedure requires.
- Weld the Q370R with low-hydrogen filler matching the base, with preheat and heat input as the qualified procedure requires for normalized fine-grain steel.
- Back-gouge from the clad side to sound base weld metal.
- Lay the transition layer with an E309MoL / ER309LMo type filler, which keeps molybdenum in the transition layer.
- Finish with E316L / ER316L filler.
- Pickle and passivate the weld zone.
Q370R is welded with low-hydrogen consumables of matching strength; heat input is controlled to keep heat-affected-zone toughness. The clad side uses a 309MoL transition layer and 316L cap.
Applications of S31603 + Q370R clad plate (NB/T 47002.1)
S31603 + Q370R NB/T 47002.1 clad plate is used in large, higher-pressure GB/T 150 vessels with chloride or acid media.
- Large reactors in coal chemical and petrochemical plants.
- High-pressure columns with 316L internals service.
- Spherical tanks and large storage vessels.
- Pharmaceutical bulk reactors.
- Hydrogenation vessels in moderate temperature zones.
- Heat exchanger shells of large diameter.
Q370R or Q345R?
Q370R saves thickness where pressure governs and the vessel is large; Q345R is cheaper per tonne and easier to source for smaller vessels.
Material certificates and quality documents
Clause 7.1.5 requires the original mill certificates of the cladding and base, complete and stamped by the mill’s inspection department. If the clad plate maker holds only copies, they must carry the stockist’s inspection stamp and a signature, and the clad plate maker is responsible for their authenticity and consistency. This is why we buy cladding and base directly from mills.
| Document or test | Content |
|---|---|
| Base and cladding mill certificates | Original, or stamped and signed copies |
| Clad plate certificate | Tests of the clad plate, UT results per plate, class code |
| Repair record | Location, area, filler and parameters of any repair |
| Packaging and marking | GB/T 247 |
| Optional | Intergranular corrosion per GB/T 4334, third-party inspection, EN 10204 3.1 or 3.2 |
Equivalent standards and grades
NB/T 47002.1 is the pressure vessel standard; GB/T 8165 is the general stainless clad plate standard. The same pairing can be ordered to either, but a GB/T 150 vessel should cite NB/T 47002.1.
| Standard | Use | Bond shear | Classes |
|---|---|---|---|
| NB/T 47002.1-2019 | Pressure vessels under GB/T 150 | 210 MPa benchmark (GB/T 150.2) | B1/B2, R1/R2 |
| GB/T 8165-2025 | General stainless clad plate and strip | 250 MPa (grades 1–2), 210 MPa (grade 3) | B/R/BR 1–3 |
| ASTM A264 / ASME SA-264 | ASME vessels | 140 MPa when specified | Class 1/3/5 |
| JIS G3601 | JIS vessels | 200 N/mm² | Class 1/2 |
| Layer | GB | ASTM / ASME | UNS | EN | JIS |
|---|---|---|---|---|---|
| Cladding | 022Cr17Ni12Mo2 (S31603) | A240 / SA-240 316L | S31603 | 1.4404 | SUS316L |
| Base | Q370R (GB/T 713.2) | SA537 Cl.1 / A737 Gr.C (approx.) | — | P390N (approx.) | SPV410 (approx.) |
For ASME Code work the nearest product is SA537 Cl.1 + 316L to ASTM A264 / ASME SA-264; for general Chinese supply the same pairing is ordered to GB/T 8165. Equivalence is approximate, so check strength, tests and class against the design code before substituting.
Why order NB/T 47002.1 S31603 + Q370R from SHH STEEL
SHH STEEL is a clad plate manufacturer in China that supplies NB/T 47002.1 plate to vessel shops working under TSG 21 and GB/T 150. For S31603 + Q370R we confirm the base heat treatment route and impact test temperature before bonding.
- We agree the class code with you before production, since it fixes the UT acceptance and the tests.
- Mill certificates of cladding and base are originals from the mills, as clause 7.1.5 asks.
- Every plate is UT scanned 100 % and marked in the NB/T format.
- Plates can be cut to head blanks and tube sheet discs.
FAQ
-
Why choose Q370R as the base for 316L clad plate?
- Its 370 MPa yield reduces wall thickness in large, higher-pressure vessels compared with Q345R.
-
Does Q370R need a technical review under NB/T 47002.1?
- No. Its minimum tensile strength, 530 MPa, is below the 540 MPa threshold that triggers a review.
-
What is the composite strength of 4 + 30 mm S31603 + Q370R?
- By the thickness-weighted method, about 339 MPa yield and 525 MPa tensile minimum.
-
What is the old name of Q370R?
- 15MnNbR.
-
What is the difference between NB/T 47002.1 and GB/T 8165?
- NB/T 47002.1 is the pressure vessel standard referenced by GB/T 150, with classes B1/B2 and R1/R2 and a total thickness of 8 mm or more. GB/T 8165 is the general stainless clad plate standard with grades 1 to 3 and B, R and BR codes.
-
What is the HS code for stainless steel clad plate?
- Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
-
What should I send for a quotation?
- NB/T 47002.1-2019, S31603 + Q370R, cladding and base thickness, class code (for example B1), size, quantity, delivery condition, extra tests and certificate type.
Request a quotation for NB/T 47002.1 316L S31603 + Q370R Stainless Steel Clad Plate
NB/T 47002.1 316L S31603 + Q370R stainless steel clad plate combines 316L cladding with the fine-grain Q370R base for large, higher-pressure GB/T 150 vessels. It is classed B1/B2, 100 % UT tested and supplied with the base in its normalized condition.
Send the thickness pair, class code, plate size and quantity to SHH STEEL, or see related plates under GB/T 8165 and ASTM A264. Availability, testing and delivery are confirmed with each quotation.
Contact: admin@steelspecs.com