NB/T 47002.1 904L S39042 + Q345R Stainless Steel Clad Plate

NB/T 47002.1 904L S39042 + Q345R stainless steel clad plate bonds super austenitic 015Cr21Ni26Mo5Cu2 to Q345R for GB/T 150 vessels handling sulfuric acid, phosphoric acid and chloride-bearing media. The copper and high nickel set it apart from 316L. SHH STEEL produces it in China by explosion welding with full UT.
Keywords
NB/T 47002.1 S39042 + Q345R, 904L + Q345R clad plate, 904L clad plate for pressure vessels, super austenitic clad plate, 015Cr21Ni26Mo5Cu2 clad
Equivalent Grades:
GB/T 8165, ASTM A264 / ASME SA-264, JIS G3601; S39042 = 904L / N08904 / 1.4539; Q345R ≈ SA516 Gr.70
Share:
General Description
Material Specification
Base and Cladding Materials
Sizes and Classes
Chemical Composition
Mechanical Properties
Heat Treatment
Bond Inspection
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is NB/T 47002.1 904L S39042 + Q345R stainless steel clad plate?

NB/T 47002.1 904L S39042 + Q345R stainless steel clad plate is a pressure vessel clad plate in which 015Cr21Ni26Mo5Cu2 (S39042) stainless steel is bonded by explosion welding or roll bonding to Q345R pressure vessel steel. It is ordered to NB/T 47002.1-2019, the energy industry standard that GB/T 150 points to for stainless steel-steel clad plate in pressure vessels. The Q345R carries the design pressure; the S39042 layer is the corrosion barrier.

It is written S39042 + Q345R or 904L + Q345R. S39042 is a super austenitic stainless steel with about 25 % nickel, 20 % chromium, 4 to 5 % molybdenum and 1 to 2 % copper. The copper gives it unusual resistance to sulfuric acid, and the molybdenum and nickel give it much better pitting and stress corrosion resistance than 316L.

NB/T 47002.1 lists S39042 among its cladding examples. As a clad plate it lets phosphate fertilizer, sulfuric acid and flue gas plants use 904L where solid plate would be prohibitively expensive.

SHH STEEL can produce S39042 + Q345R clad plate to NB/T 47002.1, marked with its class code (B1 or B2 for explosion bonded plate, R1 or R2 for roll bonded plate) and certified with the full test set. Typical claddings are 2 to 16 mm on bases from 6 mm upward.

NB/T 47002.1-2019 requirements for S39042 + Q345R

NB/T 47002.1-2019 covers clad plate with a stainless steel cladding and a carbon steel, low-alloy steel or stainless steel base, made by explosion welding or roll bonding, for pressure vessels with a total thickness of 8 mm or more. It replaced NB/T 47002.1-2009, which itself replaced JB 4733-1996, and it took effect on 1 May 2020.

What changed in the 2019 edition

  • Roll bonded plate was added, with its own limits on total thickness, base-to-cladding thickness ratio, tolerances and class codes.
  • Requirements were added for stress relief heat treatment of clad plate and the equipment used.
  • Duplex stainless claddings now need a phase ratio check in the delivered condition.
  • A side bend test was added, and the inner bend test was extended from class 1 to classes 1 and 2.
  • Visual testing to NB/T 47013.7 was added, and intergranular corrosion testing of the cladding to GB/T 4334 can be specified.

Place in the GB/T 150 system

GB/T 150.2 requires stainless steel-steel clad plate for pressure vessels to meet NB/T 47002.1, requires the design documents to state the clad plate class, and limits the unbonded ratio. If a designer chooses another clad plate standard instead, the interface shear strength must still be at least 210 MPa. The service temperature range of the clad plate must satisfy the limits for both the base and the cladding.

What the order must state

Item Example for this product
Standard number NB/T 47002.1-2019
Product name Stainless steel-steel clad plate
Cladding and base grades S39042 + Q345R
Manufacturing method and class Explosion welded class 1 (B1), or as required
Delivery condition Per GB/T 150 for the base
Dimensions Cladding + base thickness × width × length, or diameter
Weight Theoretical or actual
Additional requirements For example intergranular corrosion test, cladding surface finish

S39042 cladding and Q345R base

NB/T 47002.1 Table 2 lists the cladding and base standards. Claddings come from GB/T 24511 (pressure equipment stainless plate, now continued as GB/T 713.7), with examples S11306, S11348, S30408, S30403, S32168, S31603, S31703, S39042, S22053 and S25073. Bases come from GB/T 713 (Q245R, Q345R, 15CrMoR), GB/T 3531 (16MnDR, 09MnNiDR), the forging standards NB/T 47008, 47009 and 47010, or GB/T 24511 for stainless bases. Other grades from the listed standards may also be used.

Three rules in clause 7.1 matter in practice. Forged bases must be class III or IV forgings. A base whose specified minimum tensile strength exceeds 540 MPa needs a technical review before use. Materials from standards outside Table 2 are allowed by agreement only if their requirements, including P and S limits and impact test temperature and energy, are no lower than those of the nearest Table 2 grade.

Why 015Cr21Ni26Mo5Cu2 (S39042) is used

GB/T 4237 015Cr21Ni26Mo5Cu2 S39042 contains 19.00 to 23.00 % chromium, 23.00 to 28.00 % nickel, 4.00 to 5.00 % molybdenum and 1.00 to 2.00 % copper, with carbon held to 0.020 %. For pressure vessels it is supplied as GB/T 713.7 S39042. Its minimum PREN is about 32.

Copper is the key addition for sulfuric acid: together with high nickel it keeps the passive film stable in reducing acid over a wide concentration range. Molybdenum gives pitting resistance well above 316L, and high nickel makes the grade resistant to chloride stress corrosion cracking in most conditions where austenitic steels fail.

Because S39042 is fully austenitic, it is easy to form and has no embrittling phase problem in normal fabrication, which is an advantage over duplex when the plate must be hot formed or the vessel stress relieved.

Q345R base steel

GB/T 713 Q345R is the standard carbon-manganese pressure vessel plate in China, now covered by GB/T 713.2-2023. Its minimum yield is 345 MPa up to 16 mm and falls with thickness. It is the base in most Chinese clad vessels; GB/T 713 Q245R is used for lower stresses and GB/T 713 Q370R where higher strength is needed. Q345R is often compared with SA516 Gr.70, but the two are not interchangeable without a code check.

Design notes

904L cladding is usually 3 to 4 mm on shells. The base carries the pressure; the cladding’s 220 MPa proof strength is close to 316L, so counting it changes little.

For hot concentrated phosphoric acid with fluorides, check corrosion data carefully; nickel alloys may be needed in the most severe zones.

Dimensions, class codes and marking

Item NB/T 47002.1-2019 rule
Cladding thickness Preferably 2 – 16 mm
Base thickness 6 mm minimum
Base / cladding thickness ratio Not less than 2 for roll bonding; not less than 3 for explosion welding
Roll bonded plate Total thickness generally not over 100 mm
Explosion welded plate Area generally not over 25 m²
Larger sizes By agreement
Form Single- or double-sided; rectangular, square or round
Weight Theoretical weight allowed; stainless densities in Annex A

Each plate carries a class and a code that shows the manufacturing method: B for explosion welded plate and R for roll bonded plate, followed by the class number, for example B1, B2 or R2. Each class sets the allowable unbonded ratio and the size of individual unbonded areas. A double-sided plate states the class of each face separately.

Marking examples

The standard’s own examples show the format: (S32168+Q345R)-(3+16)×2500×8000-R2-NB/T 47002.1—2019 for 3 mm S32168 roll bonded to 16 mm Q345R, class 2; and (S30408+16MnⅢ)-(8+150)×D4000-B1-NB/T 47002.1—2019 for an explosion welded tube sheet on a class III 16Mn forging.

For this product, 4 mm S39042 explosion welded to 20 mm Q345R, 2000 × 6000 mm, class 2, is marked (S39042+Q345R)-(4+20)×2000×6000-B2-NB/T 47002.1—2019.

Chemical composition of S39042 cladding and Q345R base

Under NB/T 47002.1 the cladding is normally certified to GB/T 24511 / GB/T 713.7, the pressure equipment stainless standards, which keep the alloy ranges of the general grade and tighten some residual limits. The table shows the GB/T 4237 limits of S39042 for reference; the certificate reports the limits of the standard actually ordered.

015Cr21Ni26Mo5Cu2 (S39042) cladding

Element S39042 heat analysis, % (GB/T 4237) Permitted deviation, % Product analysis limit, %
C ≤ 0.020 +0.005 ≤ 0.025
Si ≤ 1.00 +0.05 ≤ 1.05
Mn ≤ 2.00 +0.04 ≤ 2.04
P ≤ 0.045 +0.010 ≤ 0.055
S ≤ 0.035 +0.005 ≤ 0.040
Cr 19.00 – 23.00 −0.20 / +0.25 18.80 – 23.25
Ni 23.00 – 28.00 ±0.20 22.80 – 28.20
Mo 4.00 – 5.00 ±0.10 3.90 – 5.10
Cu 1.00 – 2.00 −0.05 / +0.10 0.95 – 2.10
N ≤ 0.10 +0.01 ≤ 0.11

Q345R base steel (GB/T 713.2)

Element Q345R heat analysis, % Q345R product analysis, %
Carbon (C) 0.20 max 0.22 max
Silicon (Si) 0.55 max 0.60 max
Manganese (Mn) 1.20 – 1.70 1.15 – 1.80
Phosphorus (P) 0.025 max 0.030 max
Sulfur (S) 0.010 max 0.015 max
Chromium (Cr) 0.30 max 0.34 max
Nickel (Ni) 0.30 max 0.34 max
Copper (Cu) 0.30 max 0.34 max
Molybdenum (Mo) 0.08 max 0.09 max
Niobium (Nb) 0.050 max 0.055 max
Vanadium (V) 0.050 max 0.055 max
Titanium (Ti) 0.030 max 0.035 max
Cu + Ni + Cr + Mo 0.70 max 0.75 max

The low sulfur limit, 0.010 % by heat analysis, gives Q345R good through-thickness ductility, which helps both bonding and later welding of the clad plate.

Mechanical properties and bond tests

NB/T 47002.1 tests the clad plate as a composite. It defines the yield strength used for the composite as any one of ReH, ReL, Rp0.2, Rt0.5 or Rr0.2, taken from each layer’s own material standard, so that the base and cladding values can be combined in the calculation of the clad plate’s yield strength.

Test Purpose
Tensile test Composite strength and elongation against the calculated and base requirements
Shear test Interface bond strength; 210 MPa is the GB/T 150.2 benchmark for stainless clad plate
Inner bend Cladding in compression; required for classes 1 and 2 since 2019
Outer bend Cladding in tension; checks the cladding and the interface
Side bend Added in 2019; bends across the interface
Impact test On the base, as the base standard and GB/T 150 require

Worked example for 4 + 20 mm S39042 + Q345R: the base over 16 to 36 mm has 325 MPa minimum yield and 500 MPa minimum tensile, and S39042 has 220 and 490 MPa. The thickness-weighted average, the method used in Chinese clad plate standards, gives (4 × 220 + 20 × 325) / 24 = 308 MPa for yield and (4 × 490 + 20 × 500) / 24 = 498 MPa for tensile. Designers who do not count the cladding simply use the base values for the base thickness.

Q345R base strength by thickness

Q345R thickness, mm Yield strength min, MPa Tensile strength, MPa
3 – 16 345 510 – 640
over 16 – 36 325 500 – 630
over 36 – 60 315 490 – 620
over 60 – 100 305 490 – 620
over 100 – 150 285 480 – 610
over 150 – 200 265 470 – 600

S39042 cladding strength

Property 015Cr21Ni26Mo5Cu2 (S39042)
Proof strength Rp0.2 ≥ 220 MPa
Tensile strength Rm ≥ 490 MPa
Elongation A ≥ 35 %
Hardness ≤ 90 HRB, ≤ 200 HV

Test methods for clad plate mechanical and bend properties follow GB/T 6396; tensile tests follow GB/T 228.1 and impact tests GB/T 229.

Delivery condition and stress relief

Clause 7.2 requires clad plate to be delivered flattened and sheared or cut, with the base in the hot-rolled or heat-treated condition that GB/T 150 or JB 4732 requires for that steel. Other conditions are possible by agreement in the contract. On request the cladding surface can be blasted, polished or pickled.

Stress relief of clad plate should follow GB/T 30583. The standard notes that a stress relief below the base’s tempering temperature is generally considered not to change the base’s delivery condition.

S39042 + Q345R is delivered as clad, flattened and pickled. 904L is fully austenitic and low in carbon, so normal stress relief to GB/T 30583 is acceptable, though long holds in the 600 to 900 °C range can precipitate intermetallic phases in highly alloyed grades.

Intergranular corrosion testing to GB/T 4334 can be added on request.

Ultrasonic testing and repair of unbonded areas

Every clad plate is ultrasonically tested with 100 % scanning to NB/T 47013.3, and the bond must meet the class limits in Table 3: the length of any single unbonded indication, the area of any single unbonded zone, and the total unbonded ratio. Surfaces are checked visually to NB/T 47013.7.

Unbonded areas beyond the Table 3 limits may be repaired. The cladding over the area is removed and ground down to the base, penetrant testing confirms that the unbonded zone is gone, and a certified welder repairs it with a procedure qualified to NB/T 47014. The repair is then checked by UT, which must meet Table 3, and by penetrant testing to NB/T 47013.5-2015 class I. The repair record, with location, area, filler and welding parameters, is attached to the quality certificate.

For tube sheets cut from S39042 + Q345R plate, GB/T 151 asks for explosion clad plate to class B1, so specify B1 for any plate that will be drilled.

Typical thickness combinations of S39042 + Q345R

S39042 + Q345R clad plate is specified by cladding and base thickness, width and length, or diameter for discs. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
3 + 12 15 Thin shells
3 + 16 19 Absorber shells
4 + 20 24 Reactors
4 + 25 29 Columns
4 + 30 34 Heavier shells
5 + 40 45 Tube sheets (B1)
6 + 50 and over 56 and over Thick tube sheets
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Welding S39042 + Q345R clad plate

Pressure vessel seams in S39042 + Q345R are welded base first, then the cladding is restored. Procedures are qualified to NB/T 47014 and welding follows NB/T 47015.

  1. Prepare the bevel and strip the cladding back from the root as the procedure requires.
  2. Weld the Q345R with low-hydrogen filler matching the base.
  3. Back-gouge from the clad side to sound base weld metal.
  4. Lay the transition layer with an E309MoL type filler, or a nickel-base ENiCrMo-3 type filler where the qualified procedure requires it.
  5. Finish with E385 / ER385 (904L type) filler, or a nickel-base filler with higher molybdenum where the medium needs more margin.
  6. Pickle and passivate the weld zone.

The clad side is finished with E385 / ER385 (904L type) filler or a nickel-base filler with higher molybdenum, so the weld is at least as resistant as the cladding. Keep heat input low; 904L is more prone to hot cracking than 316L.

Applications of S39042 + Q345R clad plate (NB/T 47002.1)

S39042 + Q345R NB/T 47002.1 clad plate is used in GB/T 150 vessels exposed to sulfuric acid, phosphoric acid and aggressive chloride media.

  • Phosphoric acid reactors, evaporators and storage.
  • Sulfuric acid plant coolers and towers at moderate concentration.
  • Flue gas desulfurization absorbers.
  • Pulp bleaching equipment.
  • Pharmaceutical vessels with acid chlorides.
  • Seawater-cooled heat exchangers.

904L or 2205?

904L has the better resistance to sulfuric and phosphoric acids; 2205 is stronger and better against chloride stress corrosion cracking at moderate cost.

Material certificates and quality documents

Clause 7.1.5 requires the original mill certificates of the cladding and base, complete and stamped by the mill’s inspection department. If the clad plate maker holds only copies, they must carry the stockist’s inspection stamp and a signature, and the clad plate maker is responsible for their authenticity and consistency. This is why we buy cladding and base directly from mills.

Document or test Content
Base and cladding mill certificates Original, or stamped and signed copies
Clad plate certificate Tests of the clad plate, UT results per plate, class code
Repair record Location, area, filler and parameters of any repair
Packaging and marking GB/T 247
Optional Intergranular corrosion per GB/T 4334, third-party inspection, EN 10204 3.1 or 3.2

Equivalent standards and grades

NB/T 47002.1 is the pressure vessel standard; GB/T 8165 is the general stainless clad plate standard. The same pairing can be ordered to either, but a GB/T 150 vessel should cite NB/T 47002.1.

Standard Use Bond shear Classes
NB/T 47002.1-2019 Pressure vessels under GB/T 150 210 MPa benchmark (GB/T 150.2) B1/B2, R1/R2
GB/T 8165-2025 General stainless clad plate and strip 250 MPa (grades 1–2), 210 MPa (grade 3) B/R/BR 1–3
ASTM A264 / ASME SA-264 ASME vessels 140 MPa when specified Class 1/3/5
JIS G3601 JIS vessels 200 N/mm² Class 1/2
Layer GB ASTM / ASME UNS EN JIS
Cladding 015Cr21Ni26Mo5Cu2 (S39042) A240 / SA-240 904L N08904 1.4539 SUS890L
Base Q345R (GB/T 713.2) SA516 Gr.70 (approx.) K02700 P355GH (approx.) SGV480 (approx.)

For ASME Code work the nearest product is SA516 Gr.70 + 904L to ASTM A264 / ASME SA-264; for general Chinese supply the same pairing is ordered to GB/T 8165. Equivalence is approximate, so check strength, tests and class against the design code before substituting.

Why order NB/T 47002.1 S39042 + Q345R from SHH STEEL

SHH STEEL is a clad plate manufacturer in China that supplies NB/T 47002.1 plate to vessel shops working under TSG 21 and GB/T 150. For S39042 + Q345R we buy the 904L sheet with mill certificates showing copper and molybdenum, and keep the material separate from 316L stock.

  • We agree the class code with you before production, since it fixes the UT acceptance and the tests.
  • Mill certificates of cladding and base are originals from the mills, as clause 7.1.5 asks.
  • Every plate is UT scanned 100 % and marked in the NB/T format.
  • Plates can be cut to head blanks and tube sheet discs.

FAQ

What makes 904L cladding different from 316L?
Higher nickel and molybdenum plus 1 to 2 % copper, which give much better resistance to sulfuric and phosphoric acid and to pitting.
Is S39042 listed in NB/T 47002.1?
Yes, S39042 is one of the cladding examples in Table 2.
What is the composite strength of 4 + 20 mm S39042 + Q345R?
By the thickness-weighted method, about 308 MPa yield and 498 MPa tensile minimum.
Which filler is used for the 904L cladding?
E385 / ER385 or a nickel-base filler with higher molybdenum.
What is the difference between NB/T 47002.1 and GB/T 8165?
NB/T 47002.1 is the pressure vessel standard referenced by GB/T 150, with classes B1/B2 and R1/R2 and a total thickness of 8 mm or more. GB/T 8165 is the general stainless clad plate standard with grades 1 to 3 and B, R and BR codes.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
NB/T 47002.1-2019, S39042 + Q345R, cladding and base thickness, class code (for example B1), size, quantity, delivery condition, extra tests and certificate type.

Request a quotation for NB/T 47002.1 904L S39042 + Q345R Stainless Steel Clad Plate

NB/T 47002.1 904L S39042 + Q345R stainless steel clad plate combines super austenitic 904L cladding with Q345R for GB/T 150 pressure vessels in acid service. It is classed B1/B2, 100 % UT tested and certified with original mill certificates of both layers.

Send the thickness pair, class code, plate size and quantity to SHH STEEL, or see related plates under GB/T 8165 and ASTM A264. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X