NB/T 47002.1 304 S30408 + Q245R Stainless Steel Clad Plate

NB/T 47002.1 304 S30408 + Q245R stainless steel clad plate bonds 06Cr19Ni10 to Q245R for GB/T 150 vessels with modest pressure, thin heads and heavy forming. Q245R is softer and easier to weld than Q345R. SHH STEEL produces it in China by roll bonding or explosion welding, with class codes and 100 % UT.
Keywords
NB/T 47002.1 S30408 + Q245R, 304 + Q245R clad plate, stainless clad plate Q245R, S30408 Q245R pressure vessel, 304 clad plate for tanks
Equivalent Grades:
GB/T 8165, ASTM A264 / ASME SA-264, JIS G3601; S30408 = 304; Q245R ≈ SA516 Gr.60
Share:
General Description
Material Specification
Base and Cladding Materials
Sizes and Classes
Chemical Composition
Mechanical Properties
Heat Treatment
Bond Inspection
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is NB/T 47002.1 304 S30408 + Q245R stainless steel clad plate?

NB/T 47002.1 304 S30408 + Q245R stainless steel clad plate is a pressure vessel clad plate in which 06Cr19Ni10 (S30408) stainless steel is bonded by explosion welding or roll bonding to Q245R pressure vessel steel. It is ordered to NB/T 47002.1-2019, the energy industry standard that GB/T 150 points to for stainless steel-steel clad plate in pressure vessels. The Q245R carries the design pressure; the S30408 layer is the corrosion barrier.

It is written S30408 + Q245R, or 0Cr18Ni9 + 20R on older drawings. Q245R is listed by name in NB/T 47002.1 Table 2 and is the lower-strength carbon pressure vessel plate of GB/T 713.2. With a 304-type cladding it suits low-pressure vessels, heads pressed to deep shapes, and vessels whose wall is set by minimum thickness rather than stress.

Many food, beverage and pharmaceutical vessels in China use this pairing, ordered to NB/T 47002.1 because they are still pressure vessels under TSG 21 and GB/T 150.

SHH STEEL can produce S30408 + Q245R clad plate to NB/T 47002.1, marked with its class code (B1 or B2 for explosion bonded plate, R1 or R2 for roll bonded plate) and certified with the full test set. Typical claddings are 2 to 16 mm on bases from 6 mm upward.

NB/T 47002.1-2019 requirements for S30408 + Q245R

NB/T 47002.1-2019 covers clad plate with a stainless steel cladding and a carbon steel, low-alloy steel or stainless steel base, made by explosion welding or roll bonding, for pressure vessels with a total thickness of 8 mm or more. It replaced NB/T 47002.1-2009, which itself replaced JB 4733-1996, and it took effect on 1 May 2020.

What changed in the 2019 edition

  • Roll bonded plate was added, with its own limits on total thickness, base-to-cladding thickness ratio, tolerances and class codes.
  • Requirements were added for stress relief heat treatment of clad plate and the equipment used.
  • Duplex stainless claddings now need a phase ratio check in the delivered condition.
  • A side bend test was added, and the inner bend test was extended from class 1 to classes 1 and 2.
  • Visual testing to NB/T 47013.7 was added, and intergranular corrosion testing of the cladding to GB/T 4334 can be specified.

Place in the GB/T 150 system

GB/T 150.2 requires stainless steel-steel clad plate for pressure vessels to meet NB/T 47002.1, requires the design documents to state the clad plate class, and limits the unbonded ratio. If a designer chooses another clad plate standard instead, the interface shear strength must still be at least 210 MPa. The service temperature range of the clad plate must satisfy the limits for both the base and the cladding.

What the order must state

Item Example for this product
Standard number NB/T 47002.1-2019
Product name Stainless steel-steel clad plate
Cladding and base grades S30408 + Q245R
Manufacturing method and class Explosion welded class 1 (B1), or as required
Delivery condition Per GB/T 150 for the base
Dimensions Cladding + base thickness × width × length, or diameter
Weight Theoretical or actual
Additional requirements For example intergranular corrosion test, cladding surface finish

S30408 cladding and Q245R base

NB/T 47002.1 Table 2 lists the cladding and base standards. Claddings come from GB/T 24511 (pressure equipment stainless plate, now continued as GB/T 713.7), with examples S11306, S11348, S30408, S30403, S32168, S31603, S31703, S39042, S22053 and S25073. Bases come from GB/T 713 (Q245R, Q345R, 15CrMoR), GB/T 3531 (16MnDR, 09MnNiDR), the forging standards NB/T 47008, 47009 and 47010, or GB/T 24511 for stainless bases. Other grades from the listed standards may also be used.

Three rules in clause 7.1 matter in practice. Forged bases must be class III or IV forgings. A base whose specified minimum tensile strength exceeds 540 MPa needs a technical review before use. Materials from standards outside Table 2 are allowed by agreement only if their requirements, including P and S limits and impact test temperature and energy, are no lower than those of the nearest Table 2 grade.

Why 06Cr19Ni10 (S30408) is used

S30408 (06Cr19Ni10) is the Chinese 304: about 18 % chromium and 8 to 10.5 % nickel, with carbon up to 0.07 %. On a low-pressure vessel its job is simple: keep the product clean and the shell free of rust. It resists water, steam condensate, food acids, most organic chemicals and the atmosphere, and it can be polished to a hygienic finish.

Its weakness is chloride. Warm brines, chloride-bearing cleaning agents and evaporating splash zones can cause pitting and stress corrosion cracking. For low-pressure food and pharmaceutical vessels that are cleaned with chlorinated agents, check the cleaning regime before settling on 304 rather than 316L.

Q245R base steel

GB/T 713 Q245R is the lower-strength carbon pressure vessel plate in GB/T 713.2-2023, the successor of the old 20R and 20g grades. Its minimum yield is 245 MPa up to 16 mm, with a 400 to 520 MPa tensile range. It is chosen when the design pressure is modest, when the shell is thin enough that the strength of Q345R would not reduce the thickness, or when easier forming and lower hardness in the heat-affected zone matter more than strength.

Design notes

Run the shell calculation for both Q245R and Q345R. If the higher strength of Q345R does not reduce thickness, Q245R is cheaper and easier to form. Heads with large deformation benefit from Q245R’s lower strength and higher elongation.

Specify class B2 or R2 for shells and heads, and B1 for any part that will be drilled.

Dimensions, class codes and marking

Item NB/T 47002.1-2019 rule
Cladding thickness Preferably 2 – 16 mm
Base thickness 6 mm minimum
Base / cladding thickness ratio Not less than 2 for roll bonding; not less than 3 for explosion welding
Roll bonded plate Total thickness generally not over 100 mm
Explosion welded plate Area generally not over 25 m²
Larger sizes By agreement
Form Single- or double-sided; rectangular, square or round
Weight Theoretical weight allowed; stainless densities in Annex A

Each plate carries a class and a code that shows the manufacturing method: B for explosion welded plate and R for roll bonded plate, followed by the class number, for example B1, B2 or R2. Each class sets the allowable unbonded ratio and the size of individual unbonded areas. A double-sided plate states the class of each face separately.

Marking examples

The standard’s own examples show the format: (S32168+Q345R)-(3+16)×2500×8000-R2-NB/T 47002.1—2019 for 3 mm S32168 roll bonded to 16 mm Q345R, class 2; and (S30408+16MnⅢ)-(8+150)×D4000-B1-NB/T 47002.1—2019 for an explosion welded tube sheet on a class III 16Mn forging.

For this product, 3 mm S30408 roll bonded to 10 mm Q245R, 2000 × 8000 mm, class 2, is marked (S30408+Q245R)-(3+10)×2000×8000-R2-NB/T 47002.1—2019.

Chemical composition of S30408 cladding and Q245R base

Under NB/T 47002.1 the cladding is normally certified to GB/T 24511 / GB/T 713.7, the pressure equipment stainless standards, which keep the alloy ranges of the general grade and tighten some residual limits. The table shows the GB/T 4237 limits of S30408 for reference; the certificate reports the limits of the standard actually ordered.

06Cr19Ni10 (S30408) cladding

Element S30408 heat analysis, % (GB/T 4237) Permitted deviation, % Product analysis limit, %
C ≤ 0.07 +0.01 ≤ 0.08
Si ≤ 0.75 +0.05 ≤ 0.80
Mn ≤ 2.00 +0.04 ≤ 2.04
P ≤ 0.045 +0.010 ≤ 0.055
S ≤ 0.030 +0.005 ≤ 0.035
Cr 17.50 – 19.50 ±0.20 17.30 – 19.70
Ni 8.00 – 10.50 −0.10 at min / +0.15 at max 7.90 – 10.65
N ≤ 0.10 +0.01 ≤ 0.11

Q245R base steel (GB/T 713.2)

Element Q245R heat analysis, % Q245R product analysis, %
Carbon (C) 0.20 max 0.22 max
Silicon (Si) 0.35 max 0.40 max
Manganese (Mn) 0.50 – 1.10 0.45 – 1.20
Phosphorus (P) 0.025 max 0.030 max
Sulfur (S) 0.010 max 0.015 max
Chromium (Cr) 0.30 max 0.34 max
Nickel (Ni) 0.30 max 0.34 max
Copper (Cu) 0.30 max 0.34 max
Molybdenum (Mo) 0.08 max 0.09 max
Niobium (Nb) 0.050 max 0.055 max
Vanadium (V) 0.050 max 0.055 max
Titanium (Ti) 0.030 max 0.035 max
Cu + Ni + Cr + Mo 0.70 max 0.75 max

Q245R has the same 0.010 % sulfur limit as Q345R but much less manganese, 0.50 to 1.10 %, so its carbon equivalent is lower. That makes it the easier base to weld and to cold form.

Mechanical properties and bond tests

NB/T 47002.1 tests the clad plate as a composite. It defines the yield strength used for the composite as any one of ReH, ReL, Rp0.2, Rt0.5 or Rr0.2, taken from each layer’s own material standard, so that the base and cladding values can be combined in the calculation of the clad plate’s yield strength.

Test Purpose
Tensile test Composite strength and elongation against the calculated and base requirements
Shear test Interface bond strength; 210 MPa is the GB/T 150.2 benchmark for stainless clad plate
Inner bend Cladding in compression; required for classes 1 and 2 since 2019
Outer bend Cladding in tension; checks the cladding and the interface
Side bend Added in 2019; bends across the interface
Impact test On the base, as the base standard and GB/T 150 require

Worked example for 3 + 10 mm S30408 + Q245R: the base over 3 to 16 mm has 245 MPa minimum yield and 400 MPa minimum tensile, and S30408 has 205 and 515 MPa. The thickness-weighted average, the method used in Chinese clad plate standards, gives (3 × 205 + 10 × 245) / 13 = 236 MPa for yield and (3 × 515 + 10 × 400) / 13 = 427 MPa for tensile. Designers who do not count the cladding simply use the base values for the base thickness.

Q245R base strength by thickness

Q245R thickness, mm Yield strength min, MPa Tensile strength, MPa
3 – 16 245 400 – 520
over 16 – 36 235 400 – 520
over 36 – 60 225 400 – 520
over 60 – 100 205 390 – 510
over 100 – 150 185 380 – 500
over 150 – 250 175 370 – 490

S30408 cladding strength

Property 06Cr19Ni10 (S30408)
Proof strength Rp0.2 ≥ 205 MPa
Tensile strength Rm ≥ 515 MPa
Elongation A ≥ 40 %
Hardness ≤ 201 HBW, ≤ 92 HRB, ≤ 210 HV

Test methods for clad plate mechanical and bend properties follow GB/T 6396; tensile tests follow GB/T 228.1 and impact tests GB/T 229.

Delivery condition and stress relief

Clause 7.2 requires clad plate to be delivered flattened and sheared or cut, with the base in the hot-rolled or heat-treated condition that GB/T 150 or JB 4732 requires for that steel. Other conditions are possible by agreement in the contract. On request the cladding surface can be blasted, polished or pickled.

Stress relief of clad plate should follow GB/T 30583. The standard notes that a stress relief below the base’s tempering temperature is generally considered not to change the base’s delivery condition.

S30408 + Q245R is delivered as clad, flattened and pickled, with Q245R as rolled or normalized as GB/T 150 requires. Avoid long stress relief holds with 304 cladding; use S30403 if heat treatment is planned.

Cladding surface finish can be specified for hygienic service, for example ground or polished after pickling.

Ultrasonic testing and repair of unbonded areas

Every clad plate is ultrasonically tested with 100 % scanning to NB/T 47013.3, and the bond must meet the class limits in Table 3: the length of any single unbonded indication, the area of any single unbonded zone, and the total unbonded ratio. Surfaces are checked visually to NB/T 47013.7.

Unbonded areas beyond the Table 3 limits may be repaired. The cladding over the area is removed and ground down to the base, penetrant testing confirms that the unbonded zone is gone, and a certified welder repairs it with a procedure qualified to NB/T 47014. The repair is then checked by UT, which must meet Table 3, and by penetrant testing to NB/T 47013.5-2015 class I. The repair record, with location, area, filler and welding parameters, is attached to the quality certificate.

For tube sheets cut from S30408 + Q245R plate, GB/T 151 asks for explosion clad plate to class B1, so specify B1 for any plate that will be drilled.

Typical thickness combinations of S30408 + Q245R

S30408 + Q245R clad plate is specified by cladding and base thickness, width and length, or diameter for discs. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 6 8 Thin vessels, roll bonded
2 + 8 10 Small shells
3 + 10 13 Food and beverage vessels
3 + 12 15 Shells and heads
3 + 16 19 Heads
3 + 20 23 Heavier shells
4 + 30 34 Flanges and covers
5 + 40 and over 45 and over Tube sheets (B1)
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Welding S30408 + Q245R clad plate

Pressure vessel seams in S30408 + Q245R are welded base first, then the cladding is restored. Procedures are qualified to NB/T 47014 and welding follows NB/T 47015.

  1. Prepare the bevel and strip the cladding back from the root as the procedure requires.
  2. Weld the Q245R with low-hydrogen filler matching the base.
  3. Back-gouge from the clad side to sound base weld metal.
  4. Lay the transition layer with an E309L / ER309L type filler.
  5. Finish with E308L / ER308L, so the surface matches the 304-type cladding.
  6. Pickle and passivate the weld zone.

Q245R welds easily with standard low-hydrogen filler and rarely needs preheat in clad plate thicknesses. The clad side follows the 309L transition and 308L cap sequence.

Applications of S30408 + Q245R clad plate (NB/T 47002.1)

S30408 + Q245R NB/T 47002.1 clad plate is used in low-pressure GB/T 150 vessels with a 304-type face.

  • Food and beverage pressure tanks and fermenters.
  • Pharmaceutical receivers and holding tanks.
  • Deeply pressed heads and cones.
  • Water treatment pressure filters.
  • Low-pressure chemical vessels.
  • Small tube sheets and flanges.

Q245R or Q345R?

Q245R suits thin, low-pressure and heavily formed parts; Q345R saves weight where pressure governs the wall.

Material certificates and quality documents

Clause 7.1.5 requires the original mill certificates of the cladding and base, complete and stamped by the mill’s inspection department. If the clad plate maker holds only copies, they must carry the stockist’s inspection stamp and a signature, and the clad plate maker is responsible for their authenticity and consistency. This is why we buy cladding and base directly from mills.

Document or test Content
Base and cladding mill certificates Original, or stamped and signed copies
Clad plate certificate Tests of the clad plate, UT results per plate, class code
Repair record Location, area, filler and parameters of any repair
Packaging and marking GB/T 247
Optional Intergranular corrosion per GB/T 4334, third-party inspection, EN 10204 3.1 or 3.2

Equivalent standards and grades

NB/T 47002.1 is the pressure vessel standard; GB/T 8165 is the general stainless clad plate standard. The same pairing can be ordered to either, but a GB/T 150 vessel should cite NB/T 47002.1.

Standard Use Bond shear Classes
NB/T 47002.1-2019 Pressure vessels under GB/T 150 210 MPa benchmark (GB/T 150.2) B1/B2, R1/R2
GB/T 8165-2025 General stainless clad plate and strip 250 MPa (grades 1–2), 210 MPa (grade 3) B/R/BR 1–3
ASTM A264 / ASME SA-264 ASME vessels 140 MPa when specified Class 1/3/5
JIS G3601 JIS vessels 200 N/mm² Class 1/2
Layer GB ASTM / ASME UNS EN JIS
Cladding 06Cr19Ni10 (S30408) A240 / SA-240 304 S30400 1.4301 SUS304
Base Q245R (GB/T 713.2) SA516 Gr.60 (approx.) K02100 P265GH (approx.) SGV410 (approx.)

For ASME Code work the nearest product is SA516 Gr.60 + 304 to ASTM A264 / ASME SA-264; for general Chinese supply the same pairing is ordered to GB/T 8165. Equivalence is approximate, so check strength, tests and class against the design code before substituting.

Why order NB/T 47002.1 S30408 + Q245R from SHH STEEL

SHH STEEL is a clad plate manufacturer in China that supplies NB/T 47002.1 plate to vessel shops working under TSG 21 and GB/T 150. For S30408 + Q245R we supply thin roll bonded plate and can cut head blanks to drawing.

  • We agree the class code with you before production, since it fixes the UT acceptance and the tests.
  • Mill certificates of cladding and base are originals from the mills, as clause 7.1.5 asks.
  • Every plate is UT scanned 100 % and marked in the NB/T format.
  • Plates can be cut to head blanks and tube sheet discs.

FAQ

When is Q245R preferred over Q345R as the base?
When pressure is modest, the wall is set by minimum thickness, or heads are heavily formed.
Is Q245R listed in NB/T 47002.1?
Yes, Q245R appears by name among the GB/T 713 base materials in Table 2.
What is the composite strength of 3 + 10 mm S30408 + Q245R?
By the thickness-weighted method, about 236 MPa yield and 427 MPa tensile minimum.
Is 20R the same as Q245R?
Q245R replaced the old 20R and 20g grades in GB/T 713.
What is the difference between NB/T 47002.1 and GB/T 8165?
NB/T 47002.1 is the pressure vessel standard referenced by GB/T 150, with classes B1/B2 and R1/R2 and a total thickness of 8 mm or more. GB/T 8165 is the general stainless clad plate standard with grades 1 to 3 and B, R and BR codes.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
NB/T 47002.1-2019, S30408 + Q245R, cladding and base thickness, class code (for example B1), size, quantity, delivery condition, extra tests and certificate type.

Request a quotation for NB/T 47002.1 304 S30408 + Q245R Stainless Steel Clad Plate

NB/T 47002.1 304 S30408 + Q245R stainless steel clad plate combines 06Cr19Ni10 cladding with Q245R for low-pressure GB/T 150 vessels. It is classed B1/B2 or R1/R2 and 100 % UT tested. It is the economical choice for thin shells and formed heads.

Send the thickness pair, class code, plate size and quantity to SHH STEEL, or see related plates under GB/T 8165 and ASTM A264. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response