NB/T 47002.1 321 S32168 + Q345R Stainless Steel Clad Plate
What is NB/T 47002.1 321 S32168 + Q345R stainless steel clad plate?
NB/T 47002.1 321 S32168 + Q345R stainless steel clad plate is a pressure vessel clad plate in which 06Cr18Ni11Ti (S32168) stainless steel is bonded by explosion welding or roll bonding to Q345R pressure vessel steel. It is ordered to NB/T 47002.1-2019, the energy industry standard that GB/T 150 points to for stainless steel-steel clad plate in pressure vessels. The Q345R carries the design pressure; the S32168 layer is the corrosion barrier.
It is written S32168 + Q345R, or 1Cr18Ni9Ti + 16MnR on old drawings. S32168 is an 18-10 stainless steel stabilized with titanium: titanium ties up carbon as titanium carbide, so chromium carbides do not form at grain boundaries during welding, stress relief or service in the sensitizing range.
NB/T 47002.1 itself uses S32168 + Q345R in its first marking example, a roll bonded class 2 plate, which reflects how common the pairing is in Chinese refinery and petrochemical vessels operating at moderately high temperature.
SHH STEEL can produce S32168 + Q345R clad plate to NB/T 47002.1, marked with its class code (B1 or B2 for explosion bonded plate, R1 or R2 for roll bonded plate) and certified with the full test set. Typical claddings are 2 to 16 mm on bases from 6 mm upward.
NB/T 47002.1-2019 requirements for S32168 + Q345R
NB/T 47002.1-2019 covers clad plate with a stainless steel cladding and a carbon steel, low-alloy steel or stainless steel base, made by explosion welding or roll bonding, for pressure vessels with a total thickness of 8 mm or more. It replaced NB/T 47002.1-2009, which itself replaced JB 4733-1996, and it took effect on 1 May 2020.
What changed in the 2019 edition
- Roll bonded plate was added, with its own limits on total thickness, base-to-cladding thickness ratio, tolerances and class codes.
- Requirements were added for stress relief heat treatment of clad plate and the equipment used.
- Duplex stainless claddings now need a phase ratio check in the delivered condition.
- A side bend test was added, and the inner bend test was extended from class 1 to classes 1 and 2.
- Visual testing to NB/T 47013.7 was added, and intergranular corrosion testing of the cladding to GB/T 4334 can be specified.
Place in the GB/T 150 system
GB/T 150.2 requires stainless steel-steel clad plate for pressure vessels to meet NB/T 47002.1, requires the design documents to state the clad plate class, and limits the unbonded ratio. If a designer chooses another clad plate standard instead, the interface shear strength must still be at least 210 MPa. The service temperature range of the clad plate must satisfy the limits for both the base and the cladding.
What the order must state
| Item | Example for this product |
|---|---|
| Standard number | NB/T 47002.1-2019 |
| Product name | Stainless steel-steel clad plate |
| Cladding and base grades | S32168 + Q345R |
| Manufacturing method and class | Explosion welded class 1 (B1), or as required |
| Delivery condition | Per GB/T 150 for the base |
| Dimensions | Cladding + base thickness × width × length, or diameter |
| Weight | Theoretical or actual |
| Additional requirements | For example intergranular corrosion test, cladding surface finish |
S32168 cladding and Q345R base
NB/T 47002.1 Table 2 lists the cladding and base standards. Claddings come from GB/T 24511 (pressure equipment stainless plate, now continued as GB/T 713.7), with examples S11306, S11348, S30408, S30403, S32168, S31603, S31703, S39042, S22053 and S25073. Bases come from GB/T 713 (Q245R, Q345R, 15CrMoR), GB/T 3531 (16MnDR, 09MnNiDR), the forging standards NB/T 47008, 47009 and 47010, or GB/T 24511 for stainless bases. Other grades from the listed standards may also be used.
Three rules in clause 7.1 matter in practice. Forged bases must be class III or IV forgings. A base whose specified minimum tensile strength exceeds 540 MPa needs a technical review before use. Materials from standards outside Table 2 are allowed by agreement only if their requirements, including P and S limits and impact test temperature and energy, are no lower than those of the nearest Table 2 grade.
Why 06Cr18Ni11Ti (S32168) is used
GB/T 4237 06Cr18Ni11Ti S32168 contains 17.00 to 19.00 % chromium, 9.00 to 12.00 % nickel, up to 0.08 % carbon and titanium of at least five times the carbon content. For pressure vessels it is supplied as GB/T 713.7 S32168.
Stabilization lets S32168 keep its carbon at the standard level and still resist sensitization, which gives it slightly better strength at elevated temperature than low-carbon grades. In oxidizing media and in general petrochemical service it behaves like 304. It has no molybdenum, so it is not a chloride grade.
One practical caution: titanium carbonitrides make the polished surface less clean than 304L, and titanium does not transfer well across a welding arc. Neither matters for most process vessels, but both explain why food and pharmaceutical users prefer S30403 or S31603.
Q345R base steel
GB/T 713 Q345R is the standard carbon-manganese pressure vessel plate in China, now covered by GB/T 713.2-2023. Its minimum yield is 345 MPa up to 16 mm and falls with thickness. It is the base in most Chinese clad vessels; GB/T 713 Q245R is used for lower stresses and GB/T 713 Q370R where higher strength is needed. Q345R is often compared with SA516 Gr.70, but the two are not interchangeable without a code check.
Design notes
S32168 is chosen where the vessel runs in or passes through the 400 to 800 °C sensitizing range, or where stress relief cannot be avoided, and where the medium is mildly corrosive. Q345R limits the vessel’s maximum design temperature, so check the GB/T 150 temperature limit for the base, not just the cladding.
For hot hydrogen service a Cr-Mo base such as 15CrMoR may be needed instead of Q345R.
Dimensions, class codes and marking
| Item | NB/T 47002.1-2019 rule |
|---|---|
| Cladding thickness | Preferably 2 – 16 mm |
| Base thickness | 6 mm minimum |
| Base / cladding thickness ratio | Not less than 2 for roll bonding; not less than 3 for explosion welding |
| Roll bonded plate | Total thickness generally not over 100 mm |
| Explosion welded plate | Area generally not over 25 m² |
| Larger sizes | By agreement |
| Form | Single- or double-sided; rectangular, square or round |
| Weight | Theoretical weight allowed; stainless densities in Annex A |
Each plate carries a class and a code that shows the manufacturing method: B for explosion welded plate and R for roll bonded plate, followed by the class number, for example B1, B2 or R2. Each class sets the allowable unbonded ratio and the size of individual unbonded areas. A double-sided plate states the class of each face separately.
Marking examples
The standard’s own examples show the format: (S32168+Q345R)-(3+16)×2500×8000-R2-NB/T 47002.1—2019 for 3 mm S32168 roll bonded to 16 mm Q345R, class 2; and (S30408+16MnⅢ)-(8+150)×D4000-B1-NB/T 47002.1—2019 for an explosion welded tube sheet on a class III 16Mn forging.
The standard’s own example applies directly: 3 mm S32168 roll bonded to 16 mm Q345R, 2500 × 8000 mm, class 2, is marked (S32168+Q345R)-(3+16)×2500×8000-R2-NB/T 47002.1—2019.
Chemical composition of S32168 cladding and Q345R base
Under NB/T 47002.1 the cladding is normally certified to GB/T 24511 / GB/T 713.7, the pressure equipment stainless standards, which keep the alloy ranges of the general grade and tighten some residual limits. The table shows the GB/T 4237 limits of S32168 for reference; the certificate reports the limits of the standard actually ordered.
06Cr18Ni11Ti (S32168) cladding
| Element | S32168 heat analysis, % (GB/T 4237) | Permitted deviation, % | Product analysis limit, % |
|---|---|---|---|
| C | ≤ 0.08 | +0.01 | ≤ 0.09 |
| Si | ≤ 0.75 | +0.05 | ≤ 0.80 |
| Mn | ≤ 2.00 | +0.04 | ≤ 2.04 |
| P | ≤ 0.045 | +0.010 | ≤ 0.055 |
| S | ≤ 0.030 | +0.005 | ≤ 0.035 |
| Cr | 17.00 – 19.00 | ±0.20 | 16.80 – 19.20 |
| Ni | 9.00 – 12.00 | −0.10 at min / +0.15 at max | 8.90 – 12.15 |
| N | ≤ 0.10 | +0.01 | ≤ 0.11 |
| Ti | ≥ 5 × C | — | — |
Q345R base steel (GB/T 713.2)
| Element | Q345R heat analysis, % | Q345R product analysis, % |
|---|---|---|
| Carbon (C) | 0.20 max | 0.22 max |
| Silicon (Si) | 0.55 max | 0.60 max |
| Manganese (Mn) | 1.20 – 1.70 | 1.15 – 1.80 |
| Phosphorus (P) | 0.025 max | 0.030 max |
| Sulfur (S) | 0.010 max | 0.015 max |
| Chromium (Cr) | 0.30 max | 0.34 max |
| Nickel (Ni) | 0.30 max | 0.34 max |
| Copper (Cu) | 0.30 max | 0.34 max |
| Molybdenum (Mo) | 0.08 max | 0.09 max |
| Niobium (Nb) | 0.050 max | 0.055 max |
| Vanadium (V) | 0.050 max | 0.055 max |
| Titanium (Ti) | 0.030 max | 0.035 max |
| Cu + Ni + Cr + Mo | 0.70 max | 0.75 max |
The low sulfur limit, 0.010 % by heat analysis, gives Q345R good through-thickness ductility, which helps both bonding and later welding of the clad plate.
Mechanical properties and bond tests
NB/T 47002.1 tests the clad plate as a composite. It defines the yield strength used for the composite as any one of ReH, ReL, Rp0.2, Rt0.5 or Rr0.2, taken from each layer’s own material standard, so that the base and cladding values can be combined in the calculation of the clad plate’s yield strength.
| Test | Purpose |
|---|---|
| Tensile test | Composite strength and elongation against the calculated and base requirements |
| Shear test | Interface bond strength; 210 MPa is the GB/T 150.2 benchmark for stainless clad plate |
| Inner bend | Cladding in compression; required for classes 1 and 2 since 2019 |
| Outer bend | Cladding in tension; checks the cladding and the interface |
| Side bend | Added in 2019; bends across the interface |
| Impact test | On the base, as the base standard and GB/T 150 require |
Worked example for 3 + 16 mm S32168 + Q345R: the base over 3 to 16 mm has 345 MPa minimum yield and 510 MPa minimum tensile, and S32168 has 205 and 515 MPa. The thickness-weighted average, the method used in Chinese clad plate standards, gives (3 × 205 + 16 × 345) / 19 = 323 MPa for yield and (3 × 515 + 16 × 510) / 19 = 511 MPa for tensile. Designers who do not count the cladding simply use the base values for the base thickness.
Q345R base strength by thickness
| Q345R thickness, mm | Yield strength min, MPa | Tensile strength, MPa |
|---|---|---|
| 3 – 16 | 345 | 510 – 640 |
| over 16 – 36 | 325 | 500 – 630 |
| over 36 – 60 | 315 | 490 – 620 |
| over 60 – 100 | 305 | 490 – 620 |
| over 100 – 150 | 285 | 480 – 610 |
| over 150 – 200 | 265 | 470 – 600 |
S32168 cladding strength
| Property | 06Cr18Ni11Ti (S32168) |
|---|---|
| Proof strength Rp0.2 | ≥ 205 MPa |
| Tensile strength Rm | ≥ 515 MPa |
| Elongation A | ≥ 40 % |
| Hardness | ≤ 217 HBW, ≤ 95 HRB, ≤ 220 HV |
Test methods for clad plate mechanical and bend properties follow GB/T 6396; tensile tests follow GB/T 228.1 and impact tests GB/T 229.
Delivery condition and stress relief
Clause 7.2 requires clad plate to be delivered flattened and sheared or cut, with the base in the hot-rolled or heat-treated condition that GB/T 150 or JB 4732 requires for that steel. Other conditions are possible by agreement in the contract. On request the cladding surface can be blasted, polished or pickled.
Stress relief of clad plate should follow GB/T 30583. The standard notes that a stress relief below the base’s tempering temperature is generally considered not to change the base’s delivery condition.
S32168 + Q345R is delivered as clad, flattened and pickled. Titanium stabilization means stress relief to GB/T 30583 does not sensitize the cladding.
For service that requires the best intergranular resistance after long exposure, a stabilizing treatment of the cladding can be discussed, but it must stay compatible with the Q345R base.
Ultrasonic testing and repair of unbonded areas
Every clad plate is ultrasonically tested with 100 % scanning to NB/T 47013.3, and the bond must meet the class limits in Table 3: the length of any single unbonded indication, the area of any single unbonded zone, and the total unbonded ratio. Surfaces are checked visually to NB/T 47013.7.
Unbonded areas beyond the Table 3 limits may be repaired. The cladding over the area is removed and ground down to the base, penetrant testing confirms that the unbonded zone is gone, and a certified welder repairs it with a procedure qualified to NB/T 47014. The repair is then checked by UT, which must meet Table 3, and by penetrant testing to NB/T 47013.5-2015 class I. The repair record, with location, area, filler and welding parameters, is attached to the quality certificate.
For tube sheets cut from S32168 + Q345R plate, GB/T 151 asks for explosion clad plate to class B1, so specify B1 for any plate that will be drilled.
Typical thickness combinations of S32168 + Q345R
S32168 + Q345R clad plate is specified by cladding and base thickness, width and length, or diameter for discs. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.
| Cladding + base, mm | Total, mm | Typical use |
|---|---|---|
| 2 + 10 | 12 | Thin shells |
| 3 + 12 | 15 | Shells |
| 3 + 16 | 19 | Standard example pair |
| 3 + 20 | 23 | Reactors |
| 4 + 24 | 28 | Heavier shells |
| 4 + 30 | 34 | Columns |
| 5 + 40 | 45 | Tube sheets (B1) |
| 6 + 60 and over | 66 and over | Thick tube sheets |
| Dimension | Production range |
|---|---|
| Cladding thickness | 2 mm to 20 mm (thicker by explosion bonding on request) |
| Base steel thickness | 6 mm to 200 mm |
| Total thickness | 8 mm to 220 mm |
| Width | 1000 mm to 3000 mm; wider by explosion bonding with welded cladding |
| Length | 2000 mm to 12000 mm |
| Discs and blanks | Round tube sheet blanks and head blanks cut to drawing |
| Location | China |
Welding S32168 + Q345R clad plate
Pressure vessel seams in S32168 + Q345R are welded base first, then the cladding is restored. Procedures are qualified to NB/T 47014 and welding follows NB/T 47015.
- Prepare the bevel and strip the cladding back from the root as the procedure requires.
- Weld the Q345R with low-hydrogen filler matching the base.
- Back-gouge from the clad side to sound base weld metal.
- Lay the transition layer with an E309L / ER309L type filler.
- Finish with E347 / ER347 filler, because titanium does not transfer across the arc and niobium gives the weld the stabilization.
- Pickle and passivate the weld zone.
Titanium does not transfer well across the arc, so S32168 is capped with niobium-stabilized E347 / ER347 filler over the 309L transition. Clean the weld zone of titanium oxide films before passivation.
Applications of S32168 + Q345R clad plate (NB/T 47002.1)
S32168 + Q345R NB/T 47002.1 clad plate is used in GB/T 150 vessels running warm or stress relieved.
- Refinery hydrotreater separators and drums in moderate zones.
- Petrochemical reactors running in the sensitizing range.
- Heat exchanger shells with hot process streams.
- Ethylene and aromatics plant vessels.
- Stress-relieved columns.
- Waste heat boiler drums and components.
321 or 304L?
Both resist sensitization. S32168 keeps that resistance at higher temperatures for long times; S30403 is cheaper and easier to source and is enough for ambient-temperature service with short heat treatments.
Material certificates and quality documents
Clause 7.1.5 requires the original mill certificates of the cladding and base, complete and stamped by the mill’s inspection department. If the clad plate maker holds only copies, they must carry the stockist’s inspection stamp and a signature, and the clad plate maker is responsible for their authenticity and consistency. This is why we buy cladding and base directly from mills.
| Document or test | Content |
|---|---|
| Base and cladding mill certificates | Original, or stamped and signed copies |
| Clad plate certificate | Tests of the clad plate, UT results per plate, class code |
| Repair record | Location, area, filler and parameters of any repair |
| Packaging and marking | GB/T 247 |
| Optional | Intergranular corrosion per GB/T 4334, third-party inspection, EN 10204 3.1 or 3.2 |
Equivalent standards and grades
NB/T 47002.1 is the pressure vessel standard; GB/T 8165 is the general stainless clad plate standard. The same pairing can be ordered to either, but a GB/T 150 vessel should cite NB/T 47002.1.
| Standard | Use | Bond shear | Classes |
|---|---|---|---|
| NB/T 47002.1-2019 | Pressure vessels under GB/T 150 | 210 MPa benchmark (GB/T 150.2) | B1/B2, R1/R2 |
| GB/T 8165-2025 | General stainless clad plate and strip | 250 MPa (grades 1–2), 210 MPa (grade 3) | B/R/BR 1–3 |
| ASTM A264 / ASME SA-264 | ASME vessels | 140 MPa when specified | Class 1/3/5 |
| JIS G3601 | JIS vessels | 200 N/mm² | Class 1/2 |
| Layer | GB | ASTM / ASME | UNS | EN | JIS |
|---|---|---|---|---|---|
| Cladding | 06Cr18Ni11Ti (S32168) | A240 / SA-240 321 | S32100 | 1.4541 | SUS321 |
| Base | Q345R (GB/T 713.2) | SA516 Gr.70 (approx.) | K02700 | P355GH (approx.) | SGV480 (approx.) |
For ASME Code work the nearest product is SA516 Gr.70 + 321 to ASTM A264 / ASME SA-264; for general Chinese supply the same pairing is ordered to GB/T 8165. Equivalence is approximate, so check strength, tests and class against the design code before substituting.
Why order NB/T 47002.1 S32168 + Q345R from SHH STEEL
SHH STEEL is a clad plate manufacturer in China that supplies NB/T 47002.1 plate to vessel shops working under TSG 21 and GB/T 150. For S32168 + Q345R we supply both roll bonded R2 plate for shells and explosion welded B1 plate for tube sheets.
- We agree the class code with you before production, since it fixes the UT acceptance and the tests.
- Mill certificates of cladding and base are originals from the mills, as clause 7.1.5 asks.
- Every plate is UT scanned 100 % and marked in the NB/T format.
- Plates can be cut to head blanks and tube sheet discs.
FAQ
-
Why does NB/T 47002.1 use S32168 + Q345R in its example?
- It is one of the most common Chinese pressure vessel clad plates; the example shows a roll bonded class 2 plate marking.
-
Which filler caps S32168 cladding?
- E347 / ER347, because titanium does not transfer across the arc; niobium stabilizes the weld instead.
-
What is the composite strength of 3 + 16 mm S32168 + Q345R?
- By the thickness-weighted method, about 323 MPa yield and 511 MPa tensile minimum.
-
Is 1Cr18Ni9Ti the same as S32168?
- 1Cr18Ni9Ti is an older Chinese grade; S32168 (06Cr18Ni11Ti) is the current equivalent with lower carbon.
-
What is the difference between NB/T 47002.1 and GB/T 8165?
- NB/T 47002.1 is the pressure vessel standard referenced by GB/T 150, with classes B1/B2 and R1/R2 and a total thickness of 8 mm or more. GB/T 8165 is the general stainless clad plate standard with grades 1 to 3 and B, R and BR codes.
-
What is the HS code for stainless steel clad plate?
- Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
-
What should I send for a quotation?
- NB/T 47002.1-2019, S32168 + Q345R, cladding and base thickness, class code (for example B1), size, quantity, delivery condition, extra tests and certificate type.
Request a quotation for NB/T 47002.1 321 S32168 + Q345R Stainless Steel Clad Plate
NB/T 47002.1 321 S32168 + Q345R stainless steel clad plate combines titanium-stabilized stainless cladding with Q345R for GB/T 150 vessels running hot or stress relieved. It is classed B1/B2 or R1/R2, 100 % UT tested and marked in the NB/T format the standard itself demonstrates.
Send the thickness pair, class code, plate size and quantity to SHH STEEL, or see related plates under GB/T 8165 and ASTM A264. Availability, testing and delivery are confirmed with each quotation.
Contact: admin@steelspecs.com