GOST 14637 St5sp Steel Plate | St5sp Killed Carbon Steel Plate | GOST 14637 Steel - SHH STEEL

GOST 14637 St5sp Steel Plate | St5sp Killed Carbon Steel Plate

GOST 14637 St5sp (Ст5сп) steel plate is a killed (sp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026: it was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89. SHH STEEL produces and exports this killed grade to the ordered 2024 requirements.
Grade
St5sp
Standard
GOST 14637-2024
Deoxidation
Killed (sp)
Categories (Table 1)
1–2 (not 3–7)
Tensile strength (Table 2)
490–630 N/mm²
180° bend (Table 5)
d = 3.5a / 4.5a / 4.5a
Delivery (clause 7.1.6)
Cats 1–2: HR, TM or HT (cat 6 not listed)
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of GOST 14637 St5sp Steel Plate

GOST 14637 St5sp Steel Plate is a killed (sp) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026. It was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89.

St5sp is listed in clause 6.1. In Table 2, St5sp shares a tensile-strength cell with GOST 14637 St5ps Steel Plate (490–630 N/mm²), and yield and elongation cells are merged with GOST 14637 St5Gps Steel Plate (450–590 N/mm²). A shared yield row and a different tensile-strength cell are not interchangeability: St5sp is killed (sp). In Table 1, St5sp is listed in category 1 and category 2 only. Categories 3–7 are not listed, so impact toughness is not a specified characteristic for this grade, and category 6 is not a listed option. GOST 14637 St4ps Steel Plate and GOST 14637 St4sp Steel Plate are listed in category 3 only (KCU at +20 °C) and have a lower Table 2 tensile-strength cell (410–530 N/mm²) and different Table 5 bend diameters. State the category on the order.

SHH STEEL supplies this plate in the GOST 14637 range. We review the ordered category, delivery condition and deoxidation and the category 1–2 listing before quoting production and export requirements.

GOST 14637 St5sp Steel Plate Material Specification

The applicable product standard for this page is GOST 14637-2024. The official English title is Rolled plates from nonalloyed steel of general quality. Specifications. Orders should state that edition, the grade St5sp, the category, dimensions, quantity and any agreed options. A grade name without an edition is incomplete. The thickness and width figures below are the standard scope, not a stock promise.

Parameter Detail
Standard GOST 14637-2024; in force from 1 March 2025; replaces GOST 14637-89
Official English title Rolled plates from nonalloyed steel of general quality Specifications
Grade St5sp
Deoxidation Killed (sp), as marked by the designation
Scope, sheets Thickness 4 to 160 mm inclusive; width 500 mm and more
Scope, coils Thickness 4 to 25 mm
Dimensions and tolerances Remaining assortment requirements follow GOST 19903; state thickness accuracy and flatness on the order
Permitted inspection categories 1 or 2 only (Table 1). Categories 3–7 are not listed. Category 2 adds chemical-composition control. Impact is not a specified characteristic in either listed category
Chemical composition Shall conform to GOST 380 (clause 7.1.1.1). Category 2 adds chemical-composition control in Table 1. Clause 7.1.1.3 is not written for this grade. Numeric GOST 380 limits are not tabulated on this page
Tensile properties Table 2 for categories 1 and 2 (490–630 N/mm²). Category 6 (Table 3) is not listed
Yield strength σT Table 2 minima, by thickness band, in the cells shared with St5Gps. See Mechanical Properties
180° bend Table 5 row for St5ps, St5sp and St5Gps: d = 3.5a / 4.5a / 4.5a. Not the St2/St3 or St4 rows
Impact toughness Not a specified characteristic: categories 3–7, to which Table 4 applies, are not listed
Delivery condition Clause 7.1.6, for the listed categories 1 and 2: without heat treatment (hot-rolled), or thermomechanically treated, or heat-treated. Category 6 is not listed
Ultrasonic testing By agreement, to a class of GOST 22727; class and volume are not implied by the grade
Acceptance, marking and packaging GOST 7566, with the additions in the 2024 standard

GOST 14637 is a general-quality nonalloyed plate standard. It is not a boiler or pressure-vessel plate standard, and it is not a quality carbon structural plate standard. Do not copy figures from those systems onto a GOST 14637 order.

GOST 14637 St5sp Steel Plate Chemical Composition

Clause 7.1.1.1 of GOST 14637-2024 requires the chemical composition of the steel by ladle analysis of the ladle sample, and the permissible deviations in the finished product, to conform to GOST 380. This page does not tabulate GOST 380 heat-analysis limits. Confirm every chemistry cell against the applicable official GOST 380 table. This page is not a substitute for that table.

In Table 1, category 1 does not specify or control chemical composition; category 2 does. Order category 2 when chemistry is to be a controlled characteristic. In either listed category, ladle analysis and product deviations shall conform to GOST 380. Categories 3–7 are not listed.

Clause 7.1.1.2 permits manufacture without a lower limit on carbon and manganese, except for plate intended for shipbuilding, wagon-building or welded cylinders, provided the mechanical properties of this standard are met. State that option on the order if it is required.

On purchaser request, clause 7.1.1.4 tightens sulphur and phosphorus for categories 1–5 to S not more than 0.040 % and P not more than 0.030 %. For this grade, the request applies when a listed category (category 1 or 2) is ordered. Categories 6 and 7, for which each of these elements shall not exceed 0.025 %, are not listed for this grade. If the tighter request limits are required, state them on the order.

Clause 7.1.1.3, which allows a stated reduction of a carbon or manganese lower limit at thickness up to 10 mm for Ст3кп, Ст3пс and Ст3сп, is not written for St5sp. Do not apply that option to this grade.

For subsequent hot-dip galvanizing, clause 7.1.1.5 allows agreed silicon classes. Classes B (silicon 0.14 % to 0.25 %) and D (silicon 0.25 % to 0.35 %) are the classes written for killed (sp) steel. Class A is written for rimmed (kp) steel and is not the class for this killed grade. Galvanizing class is an agreed option, not a default.

A maximum sign is an upper limit, not a target addition. Product-analysis deviations belonging to GOST 380 must not be used to widen ladle-analysis order limits. Numeric GOST 380 element ranges are not tabulated on this page.

GOST 14637 St5sp Steel Plate Mechanical Properties

Clause 7.1.7.1 requires the tensile properties of plate in categories 1–5 and 7 to meet Table 2. For this grade, only categories 1 and 2 are listed; the Table 2 values below apply to those listed categories. Units are N/mm² for strength (the unit used in the 2024 tables) and % for elongation δ5. Table 2 heading is “not less than or within limits.”

Property Thickness Requirement (Table 2)
Tensile strength σB, N/mm² All thicknesses in the 2024 scope 490–630
Yield strength σT, N/mm² ≤20 mm ≥285
Yield strength σT, N/mm² >20 mm to 40 mm inclusive ≥275
Yield strength σT, N/mm² >40 mm to 100 mm inclusive ≥265
Yield strength σT, N/mm² >100 mm ≥255
Elongation δ5, % ≤20 mm ≥20
Elongation δ5, % >20 mm to 40 mm inclusive ≥19
Elongation δ5, % >40 mm ≥17

This Table 2 tensile-strength cell (490–630 N/mm²) is shared by St5ps and St5sp. Yield and elongation cells are merged with GOST 14637 St5Gps Steel Plate, which has a lower tensile-strength cell (450–590 N/mm²). A shared yield row and a different tensile-strength cell are not interchangeability. GOST 14637 St4ps Steel Plate and GOST 14637 St4sp Steel Plate have a lower tensile-strength cell (410–530 N/mm²). Do not take figures from those other rows, and do not take yield or tensile values from another product standard.

Table 2 footnotes that apply when the corresponding cell is a specified value include the following. For coil plate of thickness over 12 mm to 25 mm inclusive, the mechanical-property norms are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. The upper tensile-strength limit may be increased by not more than 50 N/mm² while the other mechanical-property norms are observed, and by agreement with the purchaser without limiting the upper bound. By agreement, for thickness over 20 mm, the yield value may be reduced by 10 N/mm². Table 2 also permits a stated reduction of elongation for thinner plate: for thickness up to 8 mm inclusive, by 1 % absolute for each millimetre of thickness reduction; for thickness over 8 mm, by 1 % absolute. Confirm the application of this footnote against the official table when thin plate is ordered.

By agreement between the manufacturer and the purchaser, plate of St5ps and St5sp may be supplied to Table 2 with a tensile-strength range of 490 to 640 N/mm² inclusive, in place of the grade’s own Table 2 tensile-strength cell (490–630 N/mm²). State that agreed range on the order if it is required.

Clause 7.1.8 requires the plate to withstand a 180° cold bend on a mandrel of the diameter in Table 5. At the bend there shall be no fracture, delamination or cracks.

Property Thickness (a = plate thickness) Requirement (Table 5)
180° cold bend, mandrel diameter d ≤20 mm d = 3.5a
180° cold bend, mandrel diameter d >20 mm to 40 mm inclusive d = 4.5a
180° cold bend, mandrel diameter d >40 mm d = 4.5a

These 3.5a / 4.5a / 4.5a diameters are the Table 5 row written for St5ps, St5sp and St5Gps. They are not the 1.5a / 2.5a / 2.5a diameters used for the St2 and St3 grades (except category 6), and they are not the 2.5a / 3.5a / 3.5a diameters used for St0, St4ps and St4sp. Do not take mandrel diameters from another grade’s Table 5 row. Category 6, which has a further Table 5 row, is not listed for this grade.

Impact values from Table 4 are not tabulated here: Table 4 applies to categories 3–7, which are not listed for St5sp in Table 1. Impact is not a specified characteristic in category 1 or category 2. Category 6 tensile properties (Table 3) are likewise not applicable.

GOST 14637 St5sp Steel Plate Delivery Conditions

Under clause 7.1.6, plate of categories 1–5 and 7 is manufactured without heat treatment (in the hot-rolled condition), or in the thermomechanically treated condition, or in the heat-treated condition. Category 6 is manufactured in the thermomechanically treated or heat-treated condition only; category 6 is not listed for this grade. State the required delivery condition on the order. If the condition is omitted, do not assume a heat-treated or thermomechanically treated delivery from the grade name alone; for the listed categories, which all fall in the 1–5 and 7 group, the manufacturer may supply the plate hot-rolled. Record the actual condition on the quality document.

St5sp may be ordered in category 1 or category 2 only. Categories 3–7 are not listed for this grade in Table 1. State the category on the order. Category 2 adds chemical-composition control; neither listed category specifies impact toughness. Category 6 is not a listed option. A usual hot-rolled delivery is not a substitute for an agreed thermomechanical or heat-treatment condition when the project requires one, and a category-1 or category-2 plate is not a substitute for a Table 4 impact order.

GOST 14637 St5sp Steel Plate Weldability

On purchaser request, clause 7.1.2 allows plate to be supplied with a weldability guarantee, designated in the standard as GS. That guarantee is ensured by limiting the ladle-analysis carbon content to not more than 0.22 %. If a weldability guarantee is required, state it on the order. The designation alone does not include it.

This page does not give preheat, interpass, heat-input or post-weld heat-treatment figures. The fabricator is responsible for welding-procedure qualification, consumable selection, preheat and any post-weld heat treatment required by the project specification. Do not take those figures from another standard or from a handbook and apply them as GOST 14637 rules.

St5sp is a killed (sp) steel in a higher carbon class than the St3 and St4 grades. Semi-killed and killed St5 plates, the manganese grade GOST 14637 St5Gps Steel Plate, and the St4 grades are not automatic welding substitutes for each other. Do not assume that a procedure qualified on GOST 14637 St5ps Steel Plate, on GOST 14637 St5Gps Steel Plate, or on a lower carbon class is valid for this grade without qualification. Because official GOST 380 chemistry limits are not tabulated on this page, do not assume that ladle carbon is already at or below 0.22 %. If the weldability guarantee is required, order it and confirm the carbon restriction against the official texts.

GOST 14637 St5sp Steel Plate Tolerances

Remaining assortment requirements — dimensions, shape and permissible deviations beyond the thickness and width scope in clause 6.2.1 — follow GOST 19903. State the required thickness-accuracy class, edge condition and, for plate supplied as sheets, the flatness class on the order. This page does not tabulate numerical deviation limits from GOST 19903.

Surface quality is specified in clause 7.1.3 of the 2024 standard. Defects of the types listed there are not permitted. Dressing is allowed within the depth and area limits stated in that clause; confirm those limits against the official text. Delamination on ends and on untrimmed edges is not permitted.

Ultrasonic testing is not a default requirement. By agreement, clause 7.1.9 allows plate in sheets to be supplied with ultrasonic testing to a class of GOST 22727. The continuity class and the test volume are not implied by the grade or the category; state them on the order if they are required.

GOST 14637 St5sp Steel Plate Applications and service limits

GOST 14637-2024 is a general-quality nonalloyed plate specification. Typical uses are structural and general fabrication where the ordered category, thickness and delivery condition of this grade meet the project specification. This page does not assign a service temperature, a pressure rating or a code-allowed stress from the grade name. The purchaser and the designer remain responsible for fitness for the intended duty.

St5sp is listed only in categories 1 and 2, where impact is not a specified characteristic. A higher Table 2 tensile-strength cell than St4 does not make this grade a substitute for a Table 4 impact order, and it does not qualify the plate for a pressure or low-temperature duty. Do not treat a category-1 or category-2 St5 plate as interchangeable with GOST 14637 St4ps Steel Plate or GOST 14637 St4sp Steel Plate, which are listed only in category 3. This grade is not a boiler or pressure-vessel plate and is not a quality carbon structural plate.

Compare St5sp with related GOST 14637 grades

The figures in the table below are from GOST 14637-2024 Table 2, Table 1 and Table 5. They compare grades inside this standard. A shared carbon class, a shared yield cell or a nearby tensile-strength range is not interchangeability.

Grade Table 2 tensile σB, N/mm² Yield σT, ≤20 mm Elongation δ5, ≤20 mm Table 1 categories Table 5 mandrel d
GOST 14637 St3sp Steel Plate 370–480 ≥245 ≥26 1–7 1.5a / 2.5a / 2.5a
GOST 14637 St4ps Steel Plate 410–530 ≥265 ≥24 3 only 2.5a / 3.5a / 3.5a
GOST 14637 St4sp Steel Plate 410–530 ≥265 ≥24 3 only 2.5a / 3.5a / 3.5a
GOST 14637 St5ps Steel Plate 490–630 ≥285 ≥20 1–2 3.5a / 4.5a / 4.5a
GOST 14637 St5sp Steel Plate (this page) 490–630 ≥285 ≥20 1–2 3.5a / 4.5a / 4.5a
GOST 14637 St5Gps Steel Plate 450–590 ≥285 ≥20 1–2 3.5a / 4.5a / 4.5a

St5ps and St5sp share a tensile-strength cell (490–630 N/mm²) and are listed only in categories 1 and 2. The difference is deoxidation. Yield and elongation are shared with GOST 14637 St5Gps Steel Plate, which has a lower tensile-strength cell (450–590 N/mm²). All three St5 grades use the same Table 5 mandrels (3.5a / 4.5a / 4.5a). GOST 14637 St4ps Steel Plate and GOST 14637 St4sp Steel Plate have a lower tensile-strength cell, are listed only in category 3 (with a KCU +20 °C test), and use different mandrels. A shared yield row, a higher tensile class or a shared St5 listing is not interchangeability.

Purchasers commonly compare the St5 class with GB/T 700 Q275B and EN 10025-2 S275JR. A common comparison is not an equivalent. Those grades belong to other product standards, with their own chemistry, tensile, impact and delivery rules. See also the GB/T 700 hub and the EN 10025-2 hub. Do not copy a yield, impact or chemistry figure from those pages onto a GOST 14637 order.

GOST 14637 St5sp Steel Plate Equivalent Material Grade

The entries below are commonly compared designations, not equivalent grades. GOST 14637-2024 does not publish a one-to-one equivalent-grade table for this designation. A comparable tensile class in another standard is not a substitute: chemistry, deoxidation, impact category and delivery condition must each be checked against the official texts.

Standard Country-Region Equivalent Grade Note
GB/T 700 China GB/T 700 Q275B Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.
EN 10025-2 Europe EN 10025-2 S275JR Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.

If a project specification names one of those other grades, order that specification. If it names St5sp under GOST 14637-2024, order this grade and the required category. Do not treat a cross-reference as a certified equivalent.

Why choose Us

SHH STEEL produces and exports GOST 14637 plate, including St5sp. We review the killed (sp) deoxidation, the Table 2 tensile-strength cell 490–630 N/mm², the agreed 490–640 N/mm² tensile option, the category 1–2 listing, and the Table 5 mandrels 3.5a / 4.5a / 4.5a before production, and we state the actual results on the quality document. We do not treat a shared Table 2 cell or a commonly compared foreign grade as a substitute for the ordered designation.

Orders are accepted against GOST 14637-2024. Enquiry details should include grade, category, thickness, width, length or coil mass, quantity, delivery condition and any agreed options (weldability guarantee, galvanizing class, tighter sulphur and phosphorus, ultrasonic class). See the GOST 14637 hub for the product family.

Our Service

Supply covers production to the ordered 2024 requirements, mill documentation, and export packing and shipment. Quality documents record the actual ladle analysis, tensile results and, where the category requires them, impact results, including any characteristic that Table 2 or Table 4 marks as determined for statistical data. Ultrasonic testing, a weldability guarantee and a galvanizing class are supplied when they are agreed on the order, not by default.

To enquire, state GOST 14637-2024, grade St5sp, the Table 1 category, dimensions, quantity and the required options. SHH STEEL will confirm manufacturability and the inspection plan against that order. This page is a product description; the official standard and the quality document govern acceptance.

FAQ

What is GOST 14637 St5sp steel plate?

St5sp (Ст5сп) is the killed (sp) St5 grade under GOST 14637-2024. In Table 2 it shares a tensile-strength cell with GOST 14637 St5ps Steel Plate (490–630 N/mm²), and yield and elongation with GOST 14637 St5Gps Steel Plate (which has a lower tensile-strength cell, 450–590 N/mm²). A shared cell is not interchangeability. It is listed in Table 1 categories 1 and 2 only; impact is not a specified characteristic.

Which inspection categories apply to St5sp?

Table 1 lists St5sp in category 1 and category 2 only. Categories 3–7 are not listed, so a Table 4 impact test is not a listed option, and category 6 is not listed. Category 2 adds chemical-composition control. Table 5 mandrels are d = 3.5a / 4.5a / 4.5a. State the category on the order.

What are the Table 2 tensile properties of St5sp?

Tensile strength is 490–630 N/mm². Yield minima are 285, 275, 265 and 255 N/mm², and elongation δ5 minima are 20, 19 and 17 % — the same yield and elongation cells as St5Gps, which has a different tensile-strength cell. By agreement, St5ps and St5sp may be supplied to Table 2 with a tensile-strength range of 490 to 640 N/mm² inclusive. Category 6 (Table 3) is not listed for this grade.

Is St5sp interchangeable with St5ps, St5Gps or the St4 grades?

No. GOST 14637 St5ps Steel Plate shares this tensile-strength cell but is semi-killed. GOST 14637 St5Gps Steel Plate shares yield and elongation but has a lower tensile-strength cell (450–590 N/mm²). GOST 14637 St4ps Steel Plate and GOST 14637 St4sp Steel Plate have a lower cell (410–530 N/mm²), are listed only in category 3 (with a KCU +20 °C test), and use different mandrels. A shared cell or a higher tensile class is not interchangeability.

Where is the chemical composition of St5sp specified?

Clause 7.1.1.1 requires ladle analysis and product deviations to conform to GOST 380. This page does not tabulate those GOST 380 cells. Confirm them against the applicable official GOST 380 table. Category 2 adds chemistry control in Table 1; category 1 does not. Clause 7.1.1.3 is not written for this grade. Tighter sulphur and phosphorus follow clause 7.1.1.4 when requested for a listed category.

Enquire about GOST 14637 St5sp Steel Plate

Enquire for GOST 14637 St5sp Steel Plate to GOST 14637-2024. State the category (1 or 2; categories 3–7 are not listed), thickness, width, length or coil mass, quantity, delivery condition and any agreed options. SHH STEEL will review the killed (sp) deoxidation, the Table 2 cell (490–630 N/mm²) and the Table 5 mandrels (3.5a / 4.5a / 4.5a) before quoting production and export.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response