ASTM A514 Grade B Steel Plate | A514 Gr.B 100ksi QT Structural Plate
What is ASTM A514 Grade B Steel?
ASTM A514 Grade B, also searched as A514 Gr.B, A514GRB, A514-B, A514B, T-1 Grade B and 100 ksi QT plate, is the thin-to-medium grade in ASTM A514/A514M. That book covers quenched-and-tempered alloy structural plates intended primarily for welded bridges and other structures. Maximum thickness for Grade B is 1¼ in / 32 mm. General requirements follow ASTM A6 / ASME SA-6, not A20 / SA-20.
There is no ASME SA-514 / SA-514M book in current Section II, Part A. Inquiries that write SA514 Gr.B are still buying ASTM A514 Grade B. Code quenched-and-tempered vessel plate is ASTM A517 Grade B, not A514.
This page is not Grade Q. Grade Q is the 150 mm Ni-Cr-Mo-V member. A 50 mm or 80 mm inquiry that says Grade B has to move to Grade Q, Grade E or Grade P. This page is not A572 Gr.50. A572 is Nb-V HSLA in the as-rolled or normalized condition. This page is not EN 10025-6 S690QL. S690QL is a European QT comparison, not an automatic swap.
To 32 mm, yield is 100 ksi / 690 MPa min and tensile is 110–130 ksi / 760–895 MPa. Elongation is 18% in 2 in. Hardness on plate to 20 mm is 235–293 HBW. Delivery is quenched and tempered. Grade B chemistry carries chromium, molybdenum, vanadium, titanium and boron. It does not carry the 1.20–1.50% nickel window written for Grade Q.
SHH STEEL is a global steel mill sourcing partner and steel manufacturer & exporter (mill-direct, China origin). We buy this grade from qualified Chinese mills, check Cr-Mo-V-Ti-B on the heat analysis, record QT on the certificate, and ship plate to fabricators in the USA, Europe, Middle East, Southeast Asia, Africa and South America. If the drawing is 40 mm, we will not roll Grade B and call 100 ksi enough.
Related category pages: structural steel plates, ASTM A572 / A572M and EN 10025-6.
Material Specification
| Specification Element | Requirement | SHH STEEL Compliance |
|---|---|---|
| Plate book | ASTM A514/A514M Grade B | Confirmed |
| ASME twin book | None. No SA-514 in Section II | Stated on MTC as A514 |
| Other search names | A514GRB, T-1 B, 100 ksi QT | Covered |
| Steel type | Killed QT Cr-Mo-V-Ti-B structural plate | Confirmed |
| General requirements | A6 / SA-6 | Confirmed |
| Max thickness, Grade B | 32 mm (1¼ in) | Confirmed |
| Yield to 32 mm | 690 MPa (100 ksi) min | Confirmed |
| Tensile to 32 mm | 760–895 MPa (110–130 ksi) | Confirmed |
| Supply role | Global steel mill sourcing partner | SHH STEEL |
| Certification | EN 10204 3.1 or 3.2 / third-party | As ordered |
Thick A514 sisters belong on Grade Q, Grade E and Grade P. QT vessel sisters belong on ASTM A517 Grade B and ASME SA517 Grade B. European 690 MPa QT sisters belong on EN 10025-6 S690Q and EN 10025-6 S690QL.
Chemical Composition
Grade B is the Cr-Mo-V-Ti-B member of A514. It is built for the 32 mm band. Heat analysis is the mill table. Product analysis, when ordered, follows A6 product-analysis tolerances.
Heat Analysis — ASTM A514 Grade B
| Element | Heat Analysis (%) |
|---|---|
| Carbon (C) | 0.12 – 0.21 |
| Manganese (Mn) | 0.70 – 1.00 |
| Phosphorus (P), max | 0.030 |
| Sulfur (S), max | 0.030 |
| Silicon (Si) | 0.20 – 0.35 |
| Chromium (Cr) | 0.40 – 0.65 |
| Molybdenum (Mo) | 0.15 – 0.25 |
| Vanadium (V) | 0.03 – 0.08 |
| Titanium (Ti) | 0.01 – 0.10 |
| Boron (B) | 0.0005 – 0.005 |
Nickel is not required on Grade B. Grade Q needs 1.20–1.50% Ni and 1.00–1.50% Cr. Grade E needs 1.40–2.00% Cr. Grade S has no chromium window and uses a higher manganese band. Do not accept a Q heat on a Grade B order just because both say 100 ksi. Do not accept a B heat on an 80 mm Q order. SHH STEEL prints heat analysis on every certificate. Density is 7.85 g/cm³.
Mechanical Properties
Buyers search A514 Gr.B mechanical properties, A514GRB yield, A514 B 100 ksi and T-1 Grade B tensile.
Tensile, Yield and Hardness — ASTM A514 Grade B
| Thickness | Yield min | Tensile | Elongation in 2 in, min | Hardness |
|---|---|---|---|---|
| To 20 mm (¾ in) incl. | 100 ksi / 690 MPa | 110–130 ksi / 760–895 MPa | 18% | 235–293 HBW |
| Over 20 to 32 mm (1¼ in) | 100 ksi / 690 MPa | 110–130 ksi / 760–895 MPa | 18% | — |
Grade B does not have a 65–150 mm row. That row belongs to Grade Q, Grade E and Grade P, where yield already drops to 90 ksi / 620 MPa. If the RFQ is 40 mm and the name is Grade B, the mill cannot certify A514 Grade B.
A572 Gr.50 is 345 MPa yield. ASTM A36 steel plate is 250 MPa yield. Neither is A514.
Material Comparison
| Grade | Book | Max thickness | What buyers search | Swap? |
|---|---|---|---|---|
| ASTM A514 Grade B | A514 | 32 mm | A514 Gr.B / A514GRB | This page |
| A514 Grade Q | A514 | 150 mm | A514 Gr.Q | No |
| A514 Grade E | A514 | 150 mm | A514 Gr.E | No |
| A514 Grade F | A514 | 65 mm | A514 Gr.F | No |
| A514 Grade H | A514 | 50 mm | A514 Gr.H | No |
| A514 Grade S | A514 | 65 mm | A514 Gr.S | No |
| ASTM A517 Grade B | A517 | Vessel QT | A517 Gr.B | No |
| EN 10025-6 S690QL | EN 10025-6 | S690QL | Comparison only |
Equivalent Material Grades
There is no official one-to-one worldwide swap for A514 Gr.B. What buyers compare is the 690 MPa QT structural idea in the thin-plate band.
In the United States the official plate name is ASTM A514 Grade B. Market shops still say T-1. T-1 is a product name, not the ASTM grade. Sister grades in the same book are Q, E, F, H, P and S. ASTM A517 Grade B is the vessel QT cousin under A20. Do not dual-mark A514 as A517 unless both books are fully met.
In Europe the usual comparison is EN 10025-6 S690Q or EN 10025-6 S690QL. See EN 10025-6. Those grades have their own impact tables and are not capped at 32 mm the way Grade B is. Dual marking only when both books are met.
In China there is no daily GB/T 1591 twin that copies Grade B chemistry. Q690 market plate is a strength comparison, not an automatic A514 Gr.B certificate.
| Designation | Country / region | Standard | Notes |
|---|---|---|---|
| A514 Gr.B / A514GRB / T-1 B | USA | A514 | Name on this page |
| A514 Grade Q | USA | A514 | 150 mm Ni-Cr-Mo-V |
| A514 Grade E / F / H / S | USA | A514 | Sister grades, different limits |
| ASTM A517 Grade B | USA | A517 | Vessel QT, A20 |
| EN 10025-6 S690Q | Europe | EN 10025-6 | 690 MPa QT comparison |
| EN 10025-6 S690QL | Europe | EN 10025-6 | −40 °C QT comparison |
| A572 Gr.50 | USA | A572 | 345 MPa HSLA, not QT |
100 ksi QT Structural Service
Buyers pick A514 Gr.B when a boom insert, trailer crossmember, wear-adjacent frame or light crane part wants 100 ksi yield and the plate stays inside 32 mm. Search phrases such as A514GRB, A514 Grade B, A514-B, T-1 Grade B and 100 ksi QT plate all point here.
It is the wrong plate for 80 mm chords. That work is Grade Q. It is the wrong plate for a Section VIII vessel that names SA-517. That work is ASTM A517 Grade B. It is the wrong plate for a 345 MPa frame that names A572 Gr.50.
SHH STEEL supplies this plate to fabricators in the United States, Mexico, South America, Europe, the Middle East, Africa and Asia.
Weldability
A514 Grade B is killed QT alloy structural plate at 690 MPa yield. Treat welding as production welding. Heat input, preheat and interpass have to stay inside a written WPS.
Qualify to the applicable structural code. Consumables must match a 100 ksi QT family. A procedure written for A572 Gr.50 is 345 MPa HSLA, not A514. A procedure written for Grade Q can be close in strength class, but the chemistry is not the same and the thickness band is not the same. Do not overheat the plate and then call it still Grade B. The fabricator owns the WPS. SHH STEEL can share mill heat data for that review.
Heat Treatment and Delivery Condition
Usual delivery from SHH STEEL for A514 Gr.B is quenched and tempered.
A514 does not supply Grade B as-rolled or normalized only. If the mill skipped quench and temper, the plate cannot be certified A514 Grade B.
If the job wants Charpy, write the temperature and joules. A514 does not automatically include impact. Bridge and crane files often add CVN. Extra 3.2 hold points or special NDE add time. Plan about two months when those extras are on the order.
The certificate lists ASTM A514 Grade B; heat number; heat analysis including Cr, Mo, V, Ti and B; tensile to the 32 mm table; QT delivery. Certificates may be EN 10204 3.1 or EN 10204 3.2.
Dimensions
Usual supply range from SHH STEEL for A514 Gr.B 100 ksi QT structural plate:
- Thickness: commonly 6 mm – 32 mm (Grade B max 1¼ in)
- Width: 1500 mm – 4000 mm
- Length: 3000 mm – 12000 mm
Do not order Grade B for 40 mm, 50 mm or 80 mm. Those thicknesses belong to Grade H, Grade F, Grade S, Grade E or Grade Q. Browse more sizes on the products index.
Tolerances
Dimensional limits for ASTM A514 Grade B follow ASTM A6 / ASME SA-6 unless the purchase order names another table. Do not apply pressure-vessel A20 extras unless the order writes them.
Typical thickness tolerance idea for A514 Gr.B (A6 / SA-6 reference)
| Nominal thickness (mm) | Usual minus (mm) | Usual plus (mm) |
|---|---|---|
| 6 – 10 | −0.4 | +0.8 |
| 10 – 16 | −0.4 | +0.8 |
| 16 – 25 | −0.5 | +0.9 |
| 25 – 32 | −0.6 | +1.0 |
Width on 1500–4000 mm plate is commonly held to about ±20–25 mm unless a tighter extra is named. Length on 3000–12000 mm plate is commonly held to about +50 / 0 mm or ±25 mm by mill practice. Flatness follows A6 / SA-6 unless a tighter class is written. SHH STEEL will not assume a zero-minus extra on A514GRB unless the order says so.
Supplementary Requirements
A514 Grade B already defines chemistry, QT and the 100 ksi table inside 32 mm. Extra items still have to be written on the purchase order.
Book name. Write ASTM A514 Grade B. If the inquiry said SA514, state on the PO that the mill will certify A514.
Thickness check. Confirm the ordered thickness is ≤ 32 mm before the heat is planned as Grade B.
Charpy details. Write temperature, joules, location and orientation.
Product analysis. Especially C, Cr, Mo, V, Ti, B, P and S.
Through-thickness / Z-test. Name Z15, Z25 or Z35 when needed.
NDE. A6 ultrasonic extras as named.
Hardness. The book already gives 235–293 HBW on plate to 20 mm.
Identification and stamping. Heat number, A514 Grade B, thickness and mill logo.
Third-party witness. EN 10204 3.2 with SGS, TÜV, BV, ABS, CCS, DNV or the inspector named.
Applications
| Industry | Typical components |
|---|---|
| Light crane and boom | A514 Gr.B / A514GRB inserts |
| Trailers and chassis | Grade B crossmembers from SHH STEEL |
| Mining attachments | 100 ksi QT brackets to 32 mm |
| Comparison vs Grade Q | A514GRB next to A514 Grade Q |
| Comparison vs S690 | A514GRB next to EN 10025-6 S690QL |
| Not for Code vessels | Use ASTM A517 Grade B instead |
A514 Grade B is the plate for a file that wants 100 ksi QT structural plate inside 32 mm. It is the wrong plate for 150 mm chords. That work is Grade Q. It is the wrong plate for a pressure vessel that names SA-517. That work sits on ASTM A517 Grade B. It is the wrong plate for ordinary carbon frames. That work sits on ASTM A36 steel plate or structural steel plates.
Supply Capability
SHH STEEL sources ASTM A514 Grade B from first-line Chinese mills and ships it on worldwide terms. Partner mills include Wuyang (Wugang), Angang, Shougang, Hanye, Anyang Iron & Steel, Baosteel, Xinyu, Xingcheng, Yongjin, Tsingshan, TISCO (Taiyuan), Jiuquan (JISCO), Lianzhong, Zhangpu and Baoxin, plus other qualified mills when the size or QT route requires it.
Mill test certificates are issued to EN 10204 3.1 as standard. EN 10204 3.2 is arranged when the order names a third-party hold point.
Usual stock and rolling thickness: 6 mm, 8 mm, 10 mm, 12 mm, 16 mm, 20 mm, 25 mm, 30 mm, 32 mm.
Processing: CNC or flame cutting, bevel, flattening, UT to the named class.
Trade terms: FOB Shanghai main, CIF destination available. Payment: TT, LC, or TT + LC.
Ocean time from Shanghai: US West 14–18 days; US Gulf 28–35 days; Rotterdam / Antwerp 28–35 days; Jebel Ali 18–25 days; Singapore 7–12 days; other ports quoted.
Third-party: SGS, TÜV, BV, ABS, CCS, GL, VL, DNV, RINA, NK, KR, or the inspector named.
Global Delivery & Markets
SHH STEEL is a global steel mill sourcing partner with mill partnerships in China. We supply ASTM, ASME, EN, DIN, JIS and GB steel to buyers in the United States, Europe, the Middle East, Southeast Asia, Africa and South America. Origin is mill-direct, China origin.
SHH STEEL has supplied steel plates to the USA, Mexico, Argentina, Peru, El Salvador, Spain, Netherlands, Germany, UAE, Saudi Arabia, South Africa, India, Thailand, Singapore, Vietnam, the Philippines, Japan and Korea.
Typical lead time: ex-stock 5–7 days; standard rolling / QT about 45–60 days; 3.2 inspection about 2 months.
Why Choose SHH STEEL
Experience on this grade is simple: print A514 Grade B, keep the 32 mm cap, keep QT on the certificate, and do not invent SA-514. SHH STEEL as a global steel mill sourcing partner and steel manufacturer & exporter (mill-direct, China origin) prices A514GRB from first-line mills, reports Cr-Mo-V-Ti-B chemistry, records the 100 ksi table, and issues 3.1 as standard or 3.2 when specified.
We keep the book on the order. A514GRB is not Grade Q at 80 mm. A514 Grade B is not ASTM A517 Grade B. A514 Grade B is not A572 Gr.50. If the drawing says 50 mm A514, we will move the inquiry to Grade H, Grade F or Grade Q instead of forcing Grade B.
FAQ
-
What is A514 Grade B steel plate?
- ASTM A514 Grade B, also searched as A514 Gr.B, A514GRB, A514-B and T-1 Grade B, is quenched-and-tempered alloy structural plate limited to 32 mm. Yield is 690 MPa and tensile is 760–895 MPa. SHH STEEL supplies this plate worldwide as a global steel mill sourcing partner.
-
s there an ASME SA-514 Grade B?
- No. Current Section II, Part A does not contain SA-514. The plate book is ASTM A514/A514M. Code QT vessel plate is SA-517.
-
What is the maximum thickness for A514GRB?
- 32 mm (1¼ in). Thicker plate must be Grade F, H, S, E, P or Q as the book allows
-
Can Grade B replace Grade Q?
- No. Grade Q is the 150 mm Ni-Cr-Mo-V grade. Grade B stops at 32 mm and has no nickel window.
-
How is A514 Grade B different from A517 Grade B?
- A514 is structural QT under A6. A517 is pressure-vessel QT under A20. Do not swap them.
-
What is T-1 Grade B?
- T-1 is a market name for A514-type 100 ksi QT plate. The certificate should still say ASTM A514 Grade B when that is the order.
-
Can SHH STEEL ship A514 Gr.B to the USA, Europe or the Middle East?
- es. SHH STEEL quotes FOB Shanghai and CIF to US West, US Gulf, Rotterdam, Jebel Ali, Singapore and other major ports.
-
What is the delivery time for A514 Grade B?
- Ex-stock about 5–7 days when plate is in yard. Standard mill rolling and QT about 45–60 days. 3.2 inspection about 2 months.
-
Can SHH STEEL issue EN 10204 3.2 for A514GRB?
- Yes. EN 10204 3.1 is standard. EN 10204 3.2 is arranged with SGS, TÜV, BV, ABS, CCS, DNV or the inspector named on the order.
Conclusion
ASTM A514 Grade B Steel Plate is quenched-and-tempered 100 ksi structural plate limited to 32 mm, with 690 MPa yield and 760–895 MPa tensile. Whether the inquiry says ASTM A514 Grade B, A514 Gr.B, A514GRB, A514-B, T-1 Grade B or SA514 Gr.B, SHH STEEL as a global steel mill sourcing partner and steel manufacturer & exporter (mill-direct, China origin) supplies plate with Grade B chemistry, the 32 mm A514 table, recorded QT delivery, and EN 10204 3.1 or 3.2 certification.
SHH STEEL supplies ASTM A514 Grade B / A514 Gr.B 100ksi QT Structural Plate to the USA, Mexico, South America, Europe, the Middle East, Africa and Asia for work that actually names this grade and stays inside 32 mm.
Contact SHH STEEL for mill rolling, stock inquiry, cutting, bevel, 3.2 inspection or a worldwide quotation.