ASTM A264 SA387 Gr.22 Cl.2 + 347 Stainless Steel Clad Plate

ASTM A264 SA387 Gr.22 Cl.2 + 347 clad plate bonds niobium-stabilized 347 stainless steel to a 2¼Cr-1Mo pressure vessel base. It is the classic clad combination for hydroprocessing reactors and high-pressure hydrogen vessels. SHH STEEL produces this SA387 Gr.22 Cl.2 + 347 clad plate by explosion bonding, tested after simulated PWHT when ordered.
Keywords
SA387 Gr.22 Cl.2 + 347 clad plate, 2.25Cr-1Mo clad plate, ASTM A264 347, hydroprocessing reactor clad plate, 347 clad steel
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; base ≈ 12Cr2Mo1R / 10CrMo9-10
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA387 Gr.22 Cl.2 + 347 stainless steel clad plate?

ASTM A264 SA387 Gr.22 Cl.2 + 347 stainless steel clad plate is a bimetal pressure vessel plate made of a 347 (UNS S34700) niobium-stabilized austenitic stainless steel layer metallurgically bonded to an SA387 Grade 22 Class 2 chromium-molybdenum steel base. The base steel carries pressure and structural load; the 347 face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

It is written SA387 Gr.22 Cl.2 + 347 with the thickness pair, for example 3 + 60 mm. The base is 2¼Cr-1Mo steel, the standard material for hot, high-pressure hydrogen equipment; the cladding is 347, the niobium-stabilized stainless steel used on the inside of hydrocracker and hydrotreater reactors.

Large reactors are often weld overlaid rather than clad, but for shells, heads and smaller vessels within plate size limits, an explosion clad plate gives an undiluted stainless layer that is fully inspected before fabrication.

SHH STEEL can produce 347 clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 347 clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA387 Gr.22 Cl.2 + 347
Cladding A240 / SA-240 347, UNS S34700
Base steel A387 / SA-387 Grade 22 Class 2 (chromium-molybdenum pressure vessel steel)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A complete order line reads: “Clad plate to ASME SA-264, cladding SA-240 Type 347, 3 mm minimum; base SA-387 Grade 22 Class 2, 60 mm minimum; Class 1, 100 % UT (S12); shear test required; simulated PWHT per S3 (minimum and maximum cycles); base impact tests and step-cooling as specified.”

SA387 Gr.22 Cl.2 base and 347 cladding

The two layers of SA387 Gr.22 Cl.2 + 347 are chosen for different jobs: SA387 Gr.22 Cl.2 for code strength, toughness and weldability, 347 for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 347 is specified as the cladding

347 (ASME SA240 347) contains 17.0 to 19.0 % chromium, 9.0 to 13.0 % nickel and niobium of at least 10 × C. Niobium keeps carbon tied up through the long PWHT of 2¼Cr-1Mo steel and through years of service in the sensitizing range, so the cladding resists polythionic acid stress corrosion cracking during shutdowns.

Niobium is also retained in the weld arc, so the cladding and its weld overlays have matching stabilization.

SA387 Grade 22 Class 2 as the base steel

ASME SA387 Grade 22 Class 2 is a chromium-molybdenum pressure vessel plate for elevated-temperature service. Class 2 is the higher-strength class: 515 to 690 MPa tensile and 310 MPa minimum yield, supplied normalized and tempered or, where the thickness needs it, accelerated cooled and tempered. Outside Code work it is bought as ASTM A387.

Grade 22, the 2¼Cr-1Mo steel, is the classic material for hydroprocessing reactors and high-pressure, high-temperature hydrogen equipment. It has higher creep strength and better resistance to hydrogen attack than Grade 11.

Clad plate vs weld overlay for 2¼Cr-1Mo vessels

Point 347 explosion clad plate 347 weld overlay
Chemistry at surface Full wrought 347, no dilution Diluted first layer; usually two layers
Inspection UT of bond before fabrication UT and PT after overlay
Size range Within plate size limits Any size, including forged shells
Typical use Shells, heads, drums Large reactors, nozzles

Explosion bonded and roll bonded 347 clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 347 plate is set above the SA387 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

SA387 Gr.22 bases are thick, so this combination is explosion bonded and then given the base steel’s normalizing and tempering, or stress relief, as agreed.

Chemical composition of 347 cladding and SA387 Gr.22 Cl.2 base

The chemical composition of SA387 Gr.22 Cl.2 + 347 clad plate is certified layer by layer: the 347 cladding to ASTM A240 and the base to ASTM A387 / ASME SA-387.

347 cladding (UNS S34700)

Element 347 cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.08 max 0.01 over max ≤ 0.09
Manganese (Mn) 2.00 max 0.04 over max ≤ 2.04
Phosphorus (P) 0.045 max 0.010 over max ≤ 0.055
Sulfur (S) 0.030 max 0.005 over max ≤ 0.035
Silicon (Si) 0.75 max 0.05 over max ≤ 0.80
Chromium (Cr) 17.0–19.0 0.20 under min / 0.20 over max 16.80–19.20
Nickel (Ni) 9.0–13.0 0.15 under min / 0.15 over max 8.85–13.15
Nb 10×C min, 1.00 max ratio minimum: product analysis ≥ 0.90× the specified ratio (A480 A1.1); Nb 0.05 over max ≥ 9×C; ≤ 1.05
Iron (Fe) Balance — —

These are the A240 limits for UNS S34700 with A480 product tolerances, including the 0.90 × ratio rule for niobium on product analysis.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA387 Grade 22 Class 2 base steel

Element SA387 Gr.22 Cl.2 heat analysis, % (ASTM A387)
Carbon (C) 0.05 – 0.15
Manganese (Mn) 0.30 – 0.60
Phosphorus (P) 0.025 max
Sulfur (S) 0.025 max
Silicon (Si) 0.50 max
Chromium (Cr) 2.00 – 2.50
Molybdenum (Mo) 0.90 – 1.10
Iron (Fe) Balance

These are A387 heat analysis limits; product analysis follows the A20/A20M tolerances. Cr-Mo steels are normally ordered with the A20 supplementary requirements the design code or owner specification calls for, such as impact tests and simulated PWHT.

Mechanical properties and bond strength of 347 clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 347 cladding (A240) SA387 Gr.22 Cl.2 base
Tensile strength 515 MPa min 515 – 690 MPa
Yield strength (0.2 % offset) 205 MPa min 310 MPa min
Elongation 40 % min in 50 mm 18 % min in 50 mm; reduction of area 45 % min (round) or 40 % (flat)
Hardness 201 HBW / 92 HRBW max Not specified

SA387 Gr.22 Cl.2 has a 515 MPa minimum tensile strength, so the clad plate is tested on the base only and must meet 515 to 690 MPa and 310 MPa minimum yield after simulated PWHT. Owners often specify both minimum and maximum SPWHT cycles to bracket fabrication and future repairs.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Hydroprocessing equipment is ordered Class 1 with 100 % coverage.

Heat treatment of SA387 Gr.22 Cl.2 + 347 clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

To reach Class 2 strength, the 2¼Cr-1Mo base is normalized and tempered, or accelerated cooled and tempered, after bonding. The 347 cladding goes through the same cycle; its stabilization protects it.

The vessel PWHT for 2¼Cr-1Mo is typically in the range of about 680 to 720 °C. In hot hydrogen service, stainless layers on Cr-Mo steel can disbond after rapid cooling from operating temperature; reactor owners often specify hydrogen-induced disbonding tests and controlled shutdown procedures.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 347 cladding to a minimum thickness, typically 3 mm. The 347 face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 347 clad plate

SA387 Gr.22 Cl.2 + 347 clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 347; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
3 + 30 33 Separators, drums
3 + 40 43 Exchanger shells
3 + 50 53 Vessel shells
3 + 60 63 Reactor shells within plate limits
4 + 80 84 Heads
5 + 100 105 Thick shells
6 + 120 126 Tube sheets
8 + 150 and over 158 and over Heavy sections, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA387 Gr.22 Cl.2 + 347 clad plate

A clad joint is welded as two parts: a Cr-Mo steel weld that carries the load, and an alloy overlay that restores the 347 surface. Cr-mo steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA387 Gr.22 Cl.2 side with matching 2¼Cr-1Mo low-hydrogen filler (E9018-B3 / ER90S-B3 type) with preheat.
  3. Back-gouge from the clad side to sound Cr-Mo steel weld metal.
  4. Deposit the transition layer with a 309L or 309LNb type filler.
  5. Cap with 347 filler (ER347), then pickle and passivate the weld zone.

The 2¼Cr-1Mo base is welded with matching filler, high preheat and hydrogen bake-out where specified, then PWHT. On the clad side, 309L(Nb) buffer and ER347 caps; ferrite content of the overlay is controlled to the owner’s range to balance hot cracking and sigma risk.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of SA387 Gr.22 Cl.2 + 347 clad plate

SA387 Gr.22 Cl.2 + 347 clad plate is used where hot, high-pressure hydrogen meets corrosive process streams.

  • Hydrocracker and hydrotreater separators, drums and smaller reactors.
  • Residue hydroprocessing equipment.
  • High-pressure exchanger shells and channels.
  • Hydrogen plant vessels.
  • Coal liquefaction and gasification vessels.
  • Petrochemical reactors in high-temperature hydrogen service.

Why not 321 on Grade 22?

321 is used, but 347 is preferred in severe hydroprocessing because niobium is retained in welds and the industry’s overlay experience is based on 347.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A387 and A240 347 Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Charpy and step-cooling tests of base after SPWHT; disbonding test A20/A20M and owner specification Hydroprocessing service
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 347, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 347 UNS S34700 1.4550 (X6CrNiNb18-10) SUS347 06Cr18Ni11Nb (S34778)
Base A387 / SA-387 Grade 22 Class 2 K21590 10CrMo9-10 (approx.) SCMV4 (approx.) 12Cr2Mo1R (approx.)

Chinese projects use S34778 cladding on 12Cr2Mo1R under NB/T 47002.1; Japanese projects use JIS G3601. Base equivalents are approximate; check against the design code.

Why order 347 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 2¼Cr-1Mo clad plate we plan SPWHT, impact and disbonding testing together with the vessel fabricator.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

Why is 347 used on 2¼Cr-1Mo steel?
Its niobium stabilization survives the long PWHT of 2¼Cr-1Mo steel and service in the sensitizing range, protecting against polythionic acid cracking.
How is SA387 Gr.22 Cl.2 + 347 tensile tested?
On the base only, after simulated PWHT: 515 to 690 MPa and 310 MPa minimum yield.
Should I choose clad plate or weld overlay for a reactor?
Clad plate gives undiluted, pre-inspected stainless for shells and heads within plate size limits; weld overlay covers large forged shells and nozzles.
What is hydrogen-induced disbonding?
Separation of a stainless layer from a Cr-Mo base after rapid cooling from hot hydrogen service. Owners control it with testing and shutdown procedures.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 347 cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA387 Gr.22 Cl.2 + 347 Stainless Steel Clad Plate

ASTM A264 SA387 Gr.22 Cl.2 + 347 stainless steel clad plate combines niobium-stabilized 347 with a 2¼Cr-1Mo vessel base, explosion bonded and tested after simulated PWHT, with 140 MPa shear when specified and ultrasonic Class 1, 3 or 5. It is the clad plate for hydroprocessing and high-pressure hydrogen equipment.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X