ASTM A264 SA516 Gr.70 + 2507 Super Duplex Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 2507 super duplex clad plate bonds UNS S32750 super duplex stainless steel to a carbon steel pressure vessel base. With a PREN of at least 41, it resists seawater, brines and chloride stress corrosion far beyond 316L and 2205. SHH STEEL produces it by explosion bonding with shear and ultrasonic tests when ordered.
Keywords
2507 super duplex clad plate, S32750 clad plate, ASTM A264 2507, SA516 Gr.70 + 2507, super duplex clad steel plate
Equivalent Grades:
ASME SA-264, JIS G3601, GB/T 8165, NB/T 47002.1; 2507 = S32750 / 1.4410
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A264 SA516 Gr.70 + 2507 super duplex stainless steel clad plate?

ASTM A264 SA516 Gr.70 + 2507 super duplex stainless steel clad plate is a bimetal pressure vessel plate made of a 2507 (UNS S32750) super duplex stainless steel layer metallurgically bonded to an SA516 Grade 70 carbon steel base. The base steel carries pressure and structural load; the 2507 face is the part that meets the process fluid. It is ordered to ASTM A264 or to the identical ASME Code version, SA-264.

It is written SA516 Gr.70 + 2507 or SA516 Gr.70 + S32750 with the thickness pair. 2507 is a super duplex stainless steel: about 25 % chromium, 7 % nickel, 4 % molybdenum and a high nitrogen content, in a two-phase ferrite-austenite structure. A240 requires Cr + 3.3Mo + 16N of at least 41 on the heat.

As a cladding it is chosen for seawater and hot brine service where 2205 is marginal, and where the strength and chloride stress corrosion resistance of a duplex grade are wanted rather than a nickel alloy.

SHH STEEL can produce 2507 clad plate by explosion bonding and supplies roll bonded plate where size and thickness suit that route. We make the thickness pairs that vessel shops and exchanger builders use most, certify each plate to the A264 tests written on the order, and list related products under stainless steel clad plates.

ASTM A264 / ASME SA-264 requirements for 2507 clad plate

ASTM A264 is the standard specification for stainless chromium-nickel steel-clad plate: a carbon or low-alloy steel base with a stainless layer integrally and continuously bonded to one or both faces. ASME Section II Part A reprints it as SA-264, identical with ASTM A264-12(2019). The specification has no grade list of its own; it takes the cladding chemistry from A240 and the base properties from the base steel specification.

Item Requirement for SA516 Gr.70 + 2507
Cladding A240 / SA-240 2507, UNS S32750
Base steel A516 / SA-516 Grade 70 (other carbon or low-alloy pressure vessel steels by agreement)
Bonding Explosion bonding, hot roll bonding, or any process that meets A264
General requirements A20/A20M for the base; A480/A480M for cladding product analysis
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser specifies them
Bond integrity Ultrasonic inspection to A578/A578M procedures for 10 mm and thicker; Class 1, 3 or 5
Cladding finish Blasted, pickled, blast-cleaned and pickled, or 100 % conditioned
Marking Base steel marking per A20 plus the cladding type and the specification number

A complete order line reads: “Clad plate to ASME SA-264, cladding SA-240 UNS S32750, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1, 100 % UT (S12); shear test required; ferrite measurement and ASTM A923 test of cladding as agreed.” Duplex claddings need the heat treatment agreed explicitly, because A264 leaves duplex heat treatment to agreement.

SA516 Gr.70 base and 2507 cladding

The two layers of SA516 Gr.70 + 2507 are chosen for different jobs: SA516 Gr.70 for code strength, toughness and weldability, 2507 for the corrosion duty. Because A264 certifies each layer to its own specification, the plate inherits well-known properties from both.

Why 2507 is specified as the cladding

S32750 (ASME SA240 2507) contains 24.0 to 26.0 % chromium, 6.0 to 8.0 % nickel, 3.0 to 5.0 % molybdenum and 0.24 to 0.32 % nitrogen. The PREN of at least 41 places it with the 6Mo super austenitic steels for pitting resistance, and its duplex structure gives a minimum yield of 550 MPa, far above any austenitic grade.

The cost of that performance is metallurgical sensitivity. Held between roughly 700 and 980 °C, 2507 forms sigma phase within minutes, which destroys toughness and corrosion resistance. Bonding, heat treatment and welding must all be controlled to avoid it.

SA516 Grade 70 as the base steel

ASME SA516 Grade 70 is a carbon-manganese-silicon vessel plate with 485 to 620 MPa tensile strength and 260 MPa minimum yield, supplied as-rolled or normalized and Charpy tested when the design temperature calls for it. Outside Code work the same steel is bought as ASTM A516 Grade 70; where a lower strength base is enough, ASME SA516 Grade 60 is used the same way.

2507 compared with other chloride-resistant claddings

Cladding PREN (approx.) Min. yield, MPa Choose it when
2205 (S32205) 34 450 Brackish water, moderate chlorides
2507 (S32750) 41 min 550 Seawater, hot brine, high chlorides
254SMO (S31254) 42 310 Seawater, where an austenitic grade is preferred
Alloy 625 (N06625) ~50 379 (B443 Gr1) Most severe chloride duty

Explosion bonded and roll bonded 2507 clad plate

Explosion bonding and hot roll bonding both produce the continuous metallurgical bond that A264 requires; the choice depends on thickness, plate size and quantity rather than on compliance.

Explosion bonding

The 2507 plate is set above the SA516 base at a controlled stand-off and covered with explosive. The detonation front drives the cladding into the base at an oblique angle, the surface films are jetted out, and the clean metals weld in the solid state with a wavy interface and no melting. The plate is then flattened, ultrasonically scanned and finished. This route covers thick bases, thick claddings and clad tube sheets, and A264 allows the cladding to be made from several sheets welded together when the plate is wider than the sheet.

Hot roll bonding

Cleaned stainless and carbon steel slabs are stacked, sealed and hot rolled; the reduction creates a diffusion bond. Roll bonding is efficient for large areas, thin claddings and repeat thickness pairs, but the base steel goes through the whole rolling and heat treatment cycle together with the cladding.

Point Explosion bonded Roll bonded
Bond Solid-state collision weld, wavy interface Diffusion bond formed in the mill
Best suited to Thick plates, tube sheets, project quantities Large plates, thin claddings, repeat volumes
Base steel Bought to its own specification before bonding Properties result from rolling and heat treatment of the pack
Delivery forms Plates, discs, head and tube sheet blanks Plates and wide plates

2507 is explosion bonded. Its high strength requires higher explosive loads than austenitic grades, and the bonded plate must not be given a heat treatment that passes slowly through the sigma range.

Chemical composition of 2507 cladding and SA516 Gr.70 base

The chemical composition of SA516 Gr.70 + 2507 clad plate is certified layer by layer: the 2507 cladding to ASTM A240 and the base to ASTM A516 / ASME SA-516.

2507 cladding (UNS S32750)

Element 2507 cladding, heat analysis (A240), % A480 Table A1.1 tolerance, % Product analysis limit, %
Carbon (C) 0.030 max 0.005 over max ≤ 0.035
Manganese (Mn) 1.20 max 0.04 over max ≤ 1.24
Phosphorus (P) 0.035 max 0.005 over max ≤ 0.040
Sulfur (S) 0.020 max 0.005 over max ≤ 0.025
Silicon (Si) 0.80 max 0.05 over max ≤ 0.85
Chromium (Cr) 24.0–26.0 0.25 under min / 0.25 over max 23.75–26.25
Nickel (Ni) 6.0–8.0 0.10 under min / 0.10 over max 5.90–8.10
Molybdenum (Mo) 3.0–5.0 0.10 under min / 0.10 over max 2.90–5.10
Nitrogen (N) 0.24–0.32 0.03 under min / 0.03 over max 0.21–0.35
Copper (Cu) 0.50 max 0.03 over max ≤ 0.53
Cr+3.3Mo+16N ≥ 41 (Table 1 note O) formula requirement on the heat analysis; not a Table A1.1 element —
Iron (Fe) Balance — —

These are the A240 limits for UNS S32750 with A480 product tolerances. The PREN requirement, Cr + 3.3Mo + 16N ≥ 41, applies to the heat analysis.

Product analysis of the cladding is made only when ordered. A264 asks the laboratory to remove all base metal plus 40 % of the cladding thickness from the bonded side, to a maximum of 1.6 mm, so that iron picked up at the interface does not distort the result.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength of 2507 clad plate

Mechanical testing of an A264 clad plate covers the tensile properties, the bond strength and the extent of any unbonded area, all in the final heat treated condition of the plate.

Tensile test rules in ASTM A264

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base steel minimum up to base steel maximum plus 35 MPa
Composite over 38 mm, or stronger base steel Base steel only All base steel tensile requirements
Cladding ordered as corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property 2507 cladding (A240) SA516 Gr.70 base
Tensile strength 795 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 550 MPa min 260 MPa min
Elongation 15 % min in 50 mm 21 % min in 50 mm; 17 % min in 200 mm
Hardness 310 HBW / 32 HRC max Not specified

2507 is much stronger than SA516 Gr.70. A 3 + 20 mm plate tested full thickness must still fall within 485 to 655 MPa; a high cladding ratio can push the composite towards the upper limit, so purchasers sometimes agree on base-only testing with the cladding treated as corrosion allowance.

Bond shear and bend tests

When the purchaser specifies it, the clad plate shear test must reach 20 000 psi (140 MPa). The specimen needs at least 1.9 mm of cladding, and one test represents each plate as rolled. The alternative is three bond bend tests through 180° with the cladding in compression; at least two of the three must show no more than 50 % separation on either edge. Bend specimens are 38 mm wide and not over 19 mm thick, keeping the plate’s clad-to-base ratio.

Ultrasonic bond quality classes

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

Plates 10 mm and thicker are scanned to A578/A578M procedures. If the order gives no class, Class 5 may be supplied, and scanning extent is the maker’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Seawater equipment with 2507 cladding is normally ordered Class 1 with 100 % coverage.

Heat treatment of SA516 Gr.70 + 2507 clad plate

Under ASTM A264, austenitic stainless clad plate is by default solution treated for the chromium carbides in the cladding and air cooled, unless purchaser and manufacturer agree otherwise; duplex clad plate is heat treated as agreed. Air-hardening low-alloy bases are tempered afterwards.

Super duplex clad plate is usually delivered as-clad and flattened, using solution annealed 2507 sheet. A full solution anneal of the composite at duplex temperatures, followed by rapid cooling, is difficult to apply without affecting the SA516 base; it is done only when agreed.

PWHT of the base is a particular concern. Holding 2507 at typical SA516 PWHT temperatures, around 600 to 650 °C, can begin to precipitate intermetallic phases. Avoid PWHT where the code allows, or qualify it with ASTM A923-type testing on S3 coupons.

Where the finished vessel will be post-weld heat treated, order Supplementary Requirement S3 so that the test coupons receive a simulated PWHT, and state the temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Thickness tolerances under A264 depend on whether cladding, base and total are ordered as minimum or nominal values.

Item ASTM A264 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total composite 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness ASTM A20/A20M

Order the 2507 cladding to a minimum thickness, typically 2 or 3 mm. The 2507 face is delivered blasted, pickled or fully conditioned; the steel side is supplied as bonded or shot blasted, and tube sheet faces can be machined.

Stock sizes and thickness combinations of 2507 clad plate

SA516 Gr.70 + 2507 clad plate is specified as cladding plus base thickness, then width and length. The pairs below are those we are asked for most with 2507; SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 8 10 Light tanks
2 + 10 12 Storage tanks
3 + 10 13 Low-pressure vessels
3 + 12 15 Vessel shells and heads
3 + 14 17 Process vessels
3 + 16 19 Columns, absorbers
3 + 20 23 Reactors, exchanger shells
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Small tube sheets
6 + 50 56 Tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Give the minimum cladding thickness separately from the base: “3 + 20” and “2 + 21” are both 23 mm plates but differ in price and test plan.

Welding SA516 Gr.70 + 2507 clad plate

A clad joint is welded as two parts: a carbon steel weld that carries the load, and an alloy overlay that restores the 2507 surface. Carbon steel filler must never land on the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back slightly from the root.
  2. Weld the SA516 Gr.70 side with matching carbon steel filler.
  3. Back-gouge from the clad side to sound carbon steel weld metal.
  4. Deposit the transition layer with a 309L or 309MoL type filler, or a nickel-base filler as qualified.
  5. Cap with 2509-type super duplex filler (ER2594), or a nickel-base filler such as ERNiCrMo-3, then pickle and passivate the weld zone.

Super duplex welding needs controlled heat input and interpass temperature, typically 100 to 150 °C maximum, to keep the ferrite-austenite balance and avoid intermetallics. Many projects measure ferrite on the overlay and test corrosion to ASTM G48 at an agreed temperature.

Procedures and welders are qualified to ASME Section IX, which A264 also requires for welding that forms part of the delivered plate, such as welded cladding and cladding repairs. Keep carbon steel tools and grinding discs away from the stainless face during cutting and forming.

Applications of 2507 super duplex clad plate

2507 super duplex clad plate is used where chlorides defeat 2205 and a nickel alloy would cost more than needed.

  • Seawater systems: coolers, separators and water treatment vessels offshore.
  • Desalination: reverse osmosis pressure vessels and brine equipment.
  • Oil and gas separators with high-chloride produced water.
  • Pulp bleaching with chlorine dioxide.
  • Chemical vessels with hot chloride solutions.
  • FGD absorbers with high chloride levels.

2507 or 254SMO?

Both have a PREN above 40. 2507 is stronger and resists chloride stress corrosion cracking better; 254SMO is austenitic and easier to weld and heat treat without intermetallics. Fabrication capability often decides.

Testing and certification

An A264 certificate brings the base steel tests, the bond tests and the cladding chemistry together in one report, traceable to each plate.

Test or document Basis Frequency / note
Chemical analysis of both layers A516 and A240 2507 Each heat; product analysis if ordered
Tensile test A264 and the base specification Each plate as rolled
Shear test or three bond bend tests A264 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Detection of intermetallic phases and G48 pitting test ASTM A923 and G48, by agreement When ordered
Visual and dimensional check A20 and the order Each plate
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

Weld repairs to the cladding are allowed when the defect is removed and checked by liquid penetrant, the repair procedure suits 2507, and the repair is reported on the certificate. If your project forbids repairs or wants prior approval, say so on the order.

Equivalent standards and grades

Equivalent clad plate standards describe the same kind of product but set their own test levels, so use this table to cross-check a specification rather than to swap one standard for another without review.

Standard Scope Bond shear requirement Bond quality levels
ASTM A264 / ASME SA-264 Stainless chromium-nickel steel-clad plate 140 MPa min, when specified Class 1 / 3 / 5
JIS G3601 Stainless clad steels 200 N/mm² min Per JIS G3601
GB/T 8165 Stainless steel clad plate, sheet and strip (2025 edition) 250 MPa min (grades 1 and 2); 210 MPa min (grade 3) Grades 1 / 2 / 3
NB/T 47002.1 Clad plate for pressure equipment, stainless steel-steel Per NB/T 47002.1 Per NB/T 47002.1
Layer ASTM / ASME UNS EN JIS GB
Cladding A240 / SA-240 2507 UNS S32750 1.4410 (X2CrNiMoN25-7-4) SUS327L1 022Cr25Ni7Mo4N (S25073)
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Chinese projects order the same plate to GB/T 8165 with S25073 cladding; Japanese projects use JIS G3601. Check equivalents against the design code.

Why order 2507 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying vessel shops, EPC contractors and heat exchanger builders. For 2507 orders we agree the heat treatment and the A923 or G48 testing before production.

  • We check the enquiry against ASTM A264 before quoting and flag missing items such as bond class, shear test or PWHT simulation.
  • We quote cladding and base thicknesses separately and state whether they are minimum or nominal.
  • Cladding and base steel come with traceable mill certificates, and the clad plate report includes UT maps when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut so the plate arrives ready for the next operation.

FAQ

What PREN does 2507 cladding have?
A240 requires Cr + 3.3Mo + 16N of at least 41 on the heat analysis for UNS S32750.
Is 2507 clad plate suitable for seawater?
Yes, it is one of its main uses, along with hot brines and high-chloride produced water.
Can 2507 clad plate be post-weld heat treated?
It is best avoided. PWHT temperatures can start intermetallic precipitation in super duplex; if required, qualify it on coupons with ASTM A923 testing.
Which filler metals weld SA516 Gr.70 + 2507?
Carbon steel filler for the base, a buffer such as 309L or a nickel-base alloy, then ER2594 super duplex or ERNiCrMo-3 caps.
Is ASME SA-264 the same as ASTM A264?
Yes in content. ASME publishes A264 as SA-264 in Section II Part A, identical with ASTM A264-12(2019). Order SA-264 for ASME Code vessels and A264 for other work.
What is the HS code for stainless steel clad plate?
Stainless steel clad plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
The standard (ASTM A264 or ASME SA-264), 2507 cladding thickness, base grade and thickness, minimum or nominal, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, finish and certificate type.

Request a quotation for ASTM A264 SA516 Gr.70 + 2507 Super Duplex Stainless Steel Clad Plate

ASTM A264 SA516 Gr.70 + 2507 super duplex stainless steel clad plate bonds S32750 with a PREN of at least 41 to an SA516 Grade 70 base, with 140 MPa shear when specified and ultrasonic Class 1, 3 or 5. It is the clad choice for seawater, hot brine and high-chloride service.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other grades under ASTM A264/A264M. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X