ASME SB-265 Grade 1 Titanium Plate | CP Titanium (UNS R50250)
What is ASME SB-265 Grade 1 titanium plate?
ASME SB-265 Grade 1 titanium plate is made to ASME SB-265, the ASME Boiler and Pressure Vessel Code Section II, Part B specification for titanium and titanium alloy strip, sheet and plate. It carries the UNS number R50250. Grade 1 has the lowest oxygen and iron limits of the unalloyed grades. That gives the lowest strength in the series but the best cold formability and impact toughness, which suits deep-drawn, spun and explosively clad parts.
Commercially pure titanium gets its strength from controlled interstitial levels, mainly oxygen and iron, rather than from alloying additions. It has an alpha (hexagonal) structure, cannot be hardened by heat treatment, and is normally used in the annealed condition. A stable, self-healing oxide film gives excellent resistance to seawater, brines, wet chlorine and many oxidizing acids.
Its typical density of about 4.51 g/cm³ is a little over half that of carbon steel, which is one reason titanium plate is chosen where weight matters.
Because SB-265 adopts ASTM B265, it uses the same grade numbers and UNS numbers. A grade being listed in SB-265 does not by itself mean it has allowable stresses for every Code; that depends on Section II, Part D and the Code of construction.
SHH STEEL handles Grade 1 plate enquiries within its range of titanium alloy plates and sheets, checking the ordered ASME SB-265 edition, product form and certificate type before confirming supply. Related designations covered on this site include ASTM B265 Grade 1, JIS H4600 Class 1 TP270, GB/T 3621 TA1G.
Material specification for ASME SB-265 Grade 1
ASME SB-265 is the specification for titanium and titanium alloy strip, sheet and plate in ASME Boiler and Pressure Vessel Code Section II, Part B. It adopts ASTM B265 with any ASME changes noted on its cover, so the product definitions and test requirements follow the adopted B265 edition.
| Ordering item | ASME SB-265 basis |
|---|---|
| Specification | ASME SB-265 in the BPVC Section II, Part B edition named by the Code of construction |
| Grade / UNS | Grade 1, CP Titanium, UNS R50250 |
| Product forms | Plate over 0.187 in (4.75 mm) and over 10 in (254 mm) wide; sheet and strip 0.187 in (4.75 mm) and under |
| Condition | Annealed |
| Code use | Allowable stresses, if any, come from Section II, Part D for the Code and edition being used |
| Certificate | Manufacturer’s report certifying SB-265; add ASTM B265 if dual certification is needed |
| Marking | Specification number, grade, heat number, manufacturer’s identification and nominal thickness |
The ASME edition referenced by a design may lag the newest ASTM B265 edition. If the plate will be stamped or used for Code construction, state SB-265, the Section II edition and any Code Case on the order, and confirm that the grade is accepted for the intended Code before design is fixed.
Chemical composition of ASME SB-265 Grade 1 (UNS R50250)
Single values are maximums; ranges are shown where an element is added. Titanium is the remainder. The product analysis column applies to check analysis on finished product.
| Element | Heat analysis, % | Permissible variation in product analysis, % |
|---|---|---|
| Nitrogen (N) | 0.03 | +0.02 |
| Carbon (C) | 0.08 | +0.02 |
| Hydrogen (H) | 0.015 | +0.002 |
| Iron (Fe) | 0.20 | +0.15 |
| Oxygen (O) | 0.18 | +0.03 |
| Other elements, each | 0.1 | +0.02 |
| Other elements, total | 0.4 | — |
| Titanium (Ti) | Balance | — |
The heat is analysed for the listed elements and hydrogen is reported on the final product. Residual elements need not be reported unless they exceed the each or total limits. Because SB-265 adopts B265, the limits match the ASTM grade in the adopted edition.
Mechanical properties of ASME SB-265 Grade 1
The values below are the requirements for Grade 1 plate in the annealed condition.
| Property | Requirement |
|---|---|
| Tensile strength, min | 35 ksi (240 MPa) |
| Yield strength, 0.2% offset | 20–45 ksi (138–310 MPa) |
| Elongation in 2 in or 50 mm, min | 24% |
| Bend test, under 0.070 in (1.8 mm) | Mandrel radius 1.5T, bent 105° without outside fracture |
| Bend test, 0.070–0.187 in (1.8–4.75 mm) | Mandrel radius 2T |
| Bend test, over 0.187 in (4.75 mm) | Not applicable to material over 4.75 mm |
Tensile tests are made at room temperature. The yield range has an upper limit as well as a lower one. That cap protects formability, so a plate with very high yield can fail the grade even if it is strong. Bend tests apply to sheet and strip up to 0.187 in (4.75 mm); plate over that thickness is not bend tested under the specification.
Elevated-temperature design values are not part of the plate specification. They come from the design code, such as ASME Section II, Part D where the grade is listed.
Delivery condition, finish and marking
ASME SB-265 covers material in the annealed condition. Plate must be free of injurious external and internal imperfections. Annealed product may be furnished descaled, sandblasted, ground, or sandblasted and ground; state the finish on the order.
- Condition: Annealed
- Surface: descaled, sandblasted or ground, as ordered; minor spot grinding is permitted within the thickness tolerance
- Marking: specification, grade, heat number, manufacturer’s identification and nominal thickness, in rows that can be removed with hot alkaline cleaning
- Packaging: boxed, crated, boarded or as the manufacturer’s standard practice unless the order states otherwise
CP titanium is supplied annealed; it is not strengthened by heat treatment, and stress relieving after heavy forming or welding is agreed case by case. If the plate will be formed or welded in your shop, say so at enquiry so the finish and protective packing suit the next process.
Welding and fabrication of Grade 1 titanium plate
Grade 1 is readily weldable by gas tungsten arc, plasma arc and other inert-gas processes. The key condition is shielding: hot titanium picks up oxygen, nitrogen and hydrogen from air, and that contamination embrittles the weld and heat-affected zone.
- Use trailing shields and back purging so the weld and heat-affected zone stay protected until they cool below about 400 °C
- Keep joints, filler wire and gloves clean and free of oil, moisture and iron contamination
- Use matching CP filler metal unless the design engineer specifies otherwise
- Use weld colour as a quick check of shielding quality, and reject heavily discoloured welds
- Avoid contact with carbon steel tools during cutting and forming to prevent iron pick-up
Cold forming is practical for the CP grades, with bend radii that increase as oxygen and strength rise. Springback is higher than for stainless steel, so allow for it in tooling.
For machining, use sharp carbide or high-speed steel tools, low cutting speeds, heavy feeds and plenty of coolant. CP titanium is gummy rather than hard, so dull tools cause galling and smeared surfaces. Keep chips clean and separated from other metals, and do not let fine chips accumulate, because titanium fines can ignite.
These are general practices, not a qualified procedure. The fabricator must qualify the welding procedure, filler metal and inspection to the applicable code.
Dimensional tolerances and flatness
Dimensional tolerances are set in the specification’s tables for thickness, width, length, weight and flatness. Plate flatness has its own table for annealed plate. For sheet, cold-rolled tolerances apply unless hot-rolled sheet is ordered.
State the nominal thickness, width, length, quantity and any cutting drawing at enquiry. If a project needs tighter flatness, a specific edge condition or cut-to-size pieces, write it on the order rather than relying on the default tables. No stock sizes are implied by this page.
Titanium plate can be cut by waterjet, abrasive saw, plasma or machining. Thermal cutting leaves an oxygen-enriched edge that should be removed by machining or grinding before welding or forming, so agree the cut-edge condition and any machining allowance on the order.
Applications and service limits of Grade 1 titanium plate
Typical uses of Grade 1 plate include:
- Explosion-clad and roll-bonded titanium–steel plate (cladding layer)
- Plate heat exchanger plates and deep-drawn parts
- Anodes, electrodes and electrolytic cell components
- Linings for chemical tanks and vessels where forming is severe
It has the lowest strength of the CP grades, so thicker sections may be needed than with Grade 2. Unalloyed titanium is not recommended in hydrofluoric acid or fluoride-bearing media, hot reducing acids such as concentrated hydrochloric or sulfuric acid, dry chlorine gas, or red fuming nitric acid. In hot, acidic brines where crevice corrosion is a risk, Pd-, Ru- or Ni-Mo-bearing grades are often considered instead. The design engineer must confirm suitability for the actual medium and temperature.
When selecting Grade 1, compare it with Grade 2, Grade 2H, Grade 3. The choice usually turns on the balance of strength, formability, corrosion behaviour in the actual medium and cost, and on which standard the drawing or design code names.
Compare Grade 1 with other ASME SB-265 grades
The grades below are the closest neighbours of Grade 1 in ASME SB-265. Values are tensile strength, 0.2% yield or proof strength and minimum elongation, as set by the standard.
| Grade | Tensile strength | Yield / proof strength | Elongation, min | Typical role |
|---|---|---|---|---|
| Grade 1 (R50250) | 35 ksi (240 MPa) | 20–45 ksi (138–310 MPa) | 24% | Best formability, lowest strength |
| Grade 2 (R50400) | 50 ksi (345 MPa) | 40–65 ksi (275–450 MPa) | 20% | General process equipment |
| Grade 2H (R50400) | 58 ksi (400 MPa) | 40–65 ksi (275–450 MPa) | 20% | Grade 2 with higher guaranteed tensile |
| Grade 3 (R50550) | 65 ksi (450 MPa) | 55–80 ksi (380–550 MPa) | 18% | Higher strength, less formable |
| Grade 4 (R50700) | 80 ksi (550 MPa) | 70–95 ksi (483–655 MPa) | 15% | Highest-strength CP grade |
A higher-strength CP grade is not an automatic upgrade. It reduces formability and may change bend radii and welding practice, so a grade change needs engineer approval.
ASME SB-265 Grade 1 equivalent grades
The designations below are commonly compared with ASME SB-265 Grade 1. They are close in composition and role, but limits, tests and product forms are set by each standard, so they are not automatically interchangeable.
| Standard / system | Designation | Relationship to ASME SB-265 Grade 1 |
|---|---|---|
| ASTM B265 | Grade 1 | ASTM specification adopted by SB-265; same grade requirements |
| JIS H4600 | Class 1 (TP270) | Close equivalent; JIS strength range and tests differ |
| GB/T 3621 | TA1G | Close equivalent; confirm grade name and limits in the ordered edition |
| GOST 22178 | VT1-00 | Approximate; GOST limits and sheet scope differ |
| ISO 5832-2 | Grade 1 | Implant-grade counterpart; medical scope and tighter controls |
| UNS | R50250 | Same unified number as ASTM Grade 1 |
| DIN / EN material number | 3.7025 (Ti 1) | Close CP equivalent; check the ordered European standard |
Where a drawing names one designation and the supplier offers another, agree in writing which standard governs chemistry, tensile values, testing and marking. Dual or multiple certification is possible only when the material meets every cited standard in full, and the certificate must show the results against each one.
Why choose SHH STEEL for Grade 1 titanium plate
SHH STEEL supports specification-led purchasing of titanium plate and sheet.
- We quote to ASME SB-265 and the Section II edition you name, and can arrange dual SB-265 / B265 certification
- Certificates are checked against the Grade 1 chemistry and tensile limits before shipment
- Sizes, quantities, testing and delivery are confirmed in the quotation, not assumed
- Finish, marking and packing are agreed before production
Questions on equivalents, dual certification or edition changes are answered before an order is placed.
How to enquire for ASME SB-265 Grade 1 plate
Send the material schedule with the details below. We review the enquiry and raise any open points before confirming the supply route.
| Enquiry item | Information required |
|---|---|
| Material | ASME SB-265 Grade 1 (UNS R50250), Section II edition; add ASTM B265 if dual certification |
| Product form | Plate, sheet or strip; for sheet, cold or hot rolled |
| Dimensions | Thickness, width, length, quantity and any cutting drawing |
| Finish | Descaled, sandblasted, ground or other agreed surface |
| Testing | Any special mechanical properties, extra analysis or reports |
| Documents | Certificate type and any third-party inspection |
| Destination | Delivery place and packing requirements |
FAQ
-
What is the difference between ASME SB-265 Grade 1 and ASTM B265 Grade 1?
- SB-265 adopts B265, so chemistry and tensile requirements normally match the adopted edition. SB-265 is the document cited by ASME Code construction; B265 is the ASTM industrial specification. Dual certification covers both.
-
What is the tensile strength of ASME SB-265 Grade 1 titanium plate?
- The requirement is 35 ksi (240 MPa) minimum. The 0.2% proof or yield strength is 20–45 ksi (138–310 MPa). Minimum elongation is 24%. Values apply to the condition and thickness range stated in the standard.
-
What is Grade 1 mainly used for?
- Typical uses include explosion-clad and roll-bonded titanium–steel plate (cladding layer), plate heat exchanger plates and deep-drawn parts and anodes, electrodes and electrolytic cell components. It has the lowest strength of the CP grades, so thicker sections may be needed than with Grade 2.
-
Does SB-265 use the same plate, sheet and strip definitions as B265?
- Yes. Plate is over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide; thinner product is sheet if 24 in (610 mm) or more wide, otherwise strip.
-
What should I send for a quotation?
- Send ASME SB-265 Grade 1, the edition, product form, thickness, width, length and quantity, the finish, any special testing, the certificate type and the destination.
Request a quotation for ASME SB-265 Grade 1 titanium plate
ASME SB-265 Grade 1 is CP titanium, UNS R50250, specified for 35 ksi (240 MPa) minimum tensile strength, 20–45 ksi (138–310 MPa) yield or proof strength and 24% minimum elongation in the annealed condition. Typical uses include explosion-clad and roll-bonded titanium–steel plate (cladding layer) and plate heat exchanger plates and deep-drawn parts.
Send the product form, sizes, quantity, finish, certificate type and destination to SHH STEEL. Compare other grades on the ASME SB-265 page or browse all titanium alloy plates and sheets. Availability, testing and delivery are confirmed against each enquiry.
Contact: admin@steelspecs.com