ASME SA240 UNS S31803 Stainless Steel Plate
What is ASME SA240 UNS S31803 Stainless Steel Plate?
Equivalent grades: UNS S31803 ≈ UNS S32205 ≈ EN 1.4462 X2CrNiMoN22-5-3 ≈ GB/T 022Cr22Ni5Mo3N (S22293) ≈ JIS SUS329J3L.
UNS S31803 is a duplex grade. S31803 is the original 22Cr-5Ni-3Mo-N duplex grade in A240. Its chromium, molybdenum and nitrogen ranges are wider than those of the later S32205, so a heat at the S31803 minimums has a PREN of about 30.5 against about 34 for S32205. Most plate today is melted to the S32205 window and dual-certified S31803/S32205.
ASME SA-240 is the Boiler and Pressure Vessel Code version of ASTM A240, published in Section II Part A. It is ordered when plate will be used in Code construction such as Section VIII pressure vessels, Section I boilers or B31.3 piping components made from plate. Chemistry and tensile limits are the same as in A240, but the certificate and marking must state SA-240 so the Authorized Inspector can accept the material.
This page sets out the ASME SA-240/SA-240M requirements for UNS S31803 plate: specification summary, chemistry, mechanical properties, corrosion resistance, heat treatment, finishes and tolerances, current stock, equivalents, fabrication and testing. SHH STEEL supplies it mill-direct from China with EN 10204 3.1 certificates, optional third-party inspection and in-house cutting.
UNS S31803 plate: specification summary
| Item | UNS S31803 data |
|---|---|
| Standard | ASME BPVC Section II Part A, SA-240/SA-240M (identical with or adapted from ASTM A240/A240M) |
| General requirements | SA-480/SA-480M |
| Product form | plate 5.00 mm (3/16 in.) and over; sheet and strip also covered |
| Typical thickness | 5–80 mm hot-rolled; heavier by mill enquiry |
| Widths | 1500, 2000, 2500 mm; wider by enquiry |
| Lengths | 6000 mm standard; up to 12000 mm or cut to size |
| Finish | No.1 (hot-rolled, annealed and pickled) |
| Marking | SA-240 with grade, heat and plate number; dual A240/SA-240 marking common |
| Certificates | EN 10204 3.1 stating SA-240; 3.2 with third-party or AI witness on request |
| Grade family | duplex |
Size range. Plate is produced on Steckel or reversing mills from about 5 mm up to 80–100 mm depending on grade, with widths of 1500–2500 mm and lengths up to 12 m; thinner plate of 3–12 mm is often cut from hot-rolled coil. Very heavy or wide plates, and plates with tight flatness, should be confirmed before ordering. UNS S31803 is produced regularly by several mills; common sizes are held in stock, and other sizes are rolled in the mill’s scheduled campaigns for the grade.
Chemical composition of UNS S31803 (ASME SA-240/SA-240M)
| Element | wt % |
|---|---|
| C | 0.030 max |
| Si | 1.00 max |
| Mn | 2.00 max |
| P | 0.030 max |
| S | 0.020 max |
| Cr | 21.0–23.0 |
| Ni | 4.5–6.5 |
| Mo | 2.5–3.5 |
| N | 0.08–0.20 |
Single values are maximums unless marked min. Ranges are heat (cast) analysis limits.
PREN check (Cr + 3.3 Mo + 16 N): about 30.5 at the specification minimums and about 34.1 at mid-range. Where corrosion resistance is critical, write a minimum PREN on the order and ask for the calculated value from the heat analysis on the certificate.
Mechanical properties of UNS S31803 plate
| Condition / thickness | Tensile strength, min | Yield strength 0.2 %, min | Elongation in 50 mm, min | Hardness, max |
|---|---|---|---|---|
| all thicknesses | 620 MPa (90 ksi) | 450 MPa (65 ksi) | 25 % | 293 HBW / 31 HRC |
The minimum yield strength of 450 MPa is about 2.6 times the 170 MPa minimum of ASTM 316L. Designers use this to reduce thickness, but higher strength also means higher press loads and more springback. Mill values for production heats are usually well above the minimums; use certificate values when you calculate bending forces. Tension tests are taken in the direction stated in the standard; where a hardness limit is given, it is a maximum that confirms correct annealing.
Corrosion resistance of UNS S31803: PREN and limits
Duplex steels combine about half ferrite and half austenite after solution annealing. The structure gives about twice the yield strength of 304L/316L and much better resistance to chloride stress-corrosion cracking. The PREN (Cr + 3.3 Mo + 16 N) at the specification minimum is about 30.5; a mid-range heat is about 34.1, which places the grade relative to 304L (about 18), 316L (about 24) and 2205 (about 34).
The phase balance depends on correct solution annealing and fast cooling. Too low an annealing temperature or slow cooling can precipitate sigma, chi or chromium nitrides, which cut toughness and corrosion resistance without any visible sign. That is why project specifications add ASTM A923 Method A/B/C tests and a ferrite range. Duplex grades are not recommended for long service above about 300 °C, where 475 °C embrittlement of the ferrite begins.
How UNS S31803 compares with related grades
| Grade | Cr | Ni | Mo | N | PREN (min) | YS / Rp0.2 min, MPa |
|---|---|---|---|---|---|---|
| UNS S31803 | 21.0–23.0 | 4.5–6.5 | 2.5–3.5 | 0.08–0.20 | 30.5 | 450 |
| UNS S82441 | 23.0–25.0 | 3.0–4.5 | 1.00–2.00 | 0.20–0.30 | 29.5 | 540 |
| UNS S32003 | 19.5–22.5 | 3.0–4.0 | 1.50–2.00 | 0.14–0.20 | 26.7 | 485 |
| UNS S32202 | 21.5–24.0 | 1.00–2.80 | 0.45 max | 0.18–0.26 | 24.4 | 450 |
| UNS S32900 | 23.0–28.0 | 2.0–5.0 | 1.00–2.00 | — | 26.3 | 485 |
Choose UNS S31803 when you need more strength and chloride stress-corrosion resistance than 316L at lower cost than super-austenitic or super-duplex grades. Do not use it for long-term service above about 300 °C or where full non-magnetic behaviour is required.
The table uses specification limits, not typical mill values, so it shows the guaranteed position of each grade. Final selection should also consider product availability in the thickness you need, welding consumables, and the inspection requirements of your project.
Heat treatment and delivery condition of UNS S31803
Heat treatment: 1020–1100 °C, rapid cooling.
Rapid cooling from the solution-anneal temperature is essential to avoid sigma, chi and chromium nitrides in the 700–1000 °C range. Stress relieving in that range is not allowed; any hot forming must be followed by a full solution anneal and quench.
Surface finishes for UNS S31803 plate
Plate to SA-240 is normally supplied with a No.1 finish: hot rolled, solution annealed and pickled, with a matt grey surface. Shot-blasted and pickled surfaces are the norm on heavy plate. Ground or polished faces, and plates with protective film for the process side, can be produced after delivery in our workshop. Surface defects are judged against the A480/SA-480 workmanship clause; for vessel internals the purchaser may add surface-roughness or cleanliness requirements.
Dimensions, tolerances and flatness
Thickness, width, length, flatness and camber tolerances follow SA-480/A480 tables for hot-rolled plate; ordered thickness is a minimum unless the order states nominal. For pressure parts, the thickness at any point must not fall below the ordered minimum, so heavy plate is often ordered with a small plus allowance. Flatness of thin plate cut from coil should be checked after cutting. Mill edge, sheared, plasma or waterjet-cut edges and bevelling for welding are available.
Code use of SA-240 plate. Before welding, the manufacturer must identify the P-Number and group number of S31803 from ASME Section IX (QW/QG-422) for the welding procedure qualification, and the designer takes allowable stresses from Section II Part D. Impact-test exemptions for austenitic and duplex plate are given in Section VIII Division 1 (UHA-51) and depend on grade, thickness and minimum design metal temperature, so cryogenic or low-temperature duty should be stated when you order. For heavy plate, ultrasonic examination to SA-578 and PMI of each plate are common supplementary requirements. Ask for the plate number to be hard-stamped or stencilled so traceability survives cutting.
UNS S31803 plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Finish | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1500 / 2000 | 6000 | No.1 | 200+ t | China |
| 8 | 1500 / 2000 | 6000 | No.1 | 200+ t | China |
| 10 | 2000 | 6000 | No.1 | 100+ t | China |
| 12 | 2000 | 6000 | No.1 | 100+ t | China |
| 16 | 2000 / 2500 | 6000 | No.1 | 100+ t | China |
| 20 | 2000 / 2500 | 6000 / 8000 | No.1 | 100+ t | China |
| 30 | 2000 / 2500 | 6000 | No.1 | 100+ t | China |
Quantities are approximate and stock changes daily. Send your size list for current availability; other thicknesses, widths and cut sizes can be supplied from mill production.
Packing and logistics. Plate is bundled on steel or wooden skids with steel bands and edge protection, typically 3–8 t per bundle, and marked with heat and plate numbers. Cut pieces are crated. Heavy and wide plate ships in open-top or flat-rack containers or by break-bulk; we send loading photos with the shipping documents.
UNS S31803 equivalents in other standards
| Standard | Designation | Comment |
|---|---|---|
| ASTM / UNS | UNS S32205 | same alloy family and limits closely matched; compare each limit on the certificate |
| EN | 1.4462 X2CrNiMoN22-5-3 | same alloy family and limits closely matched; compare each limit on the certificate |
| GB/T | 022Cr22Ni5Mo3N (S22293) | same alloy family and limits closely matched; compare each limit on the certificate |
| JIS | SUS329J3L | same alloy family and limits closely matched; compare each limit on the certificate |
Equivalents are close, not identical. When a project names one standard, order to that standard or ask for multiple certification and check every limit on the certificate.
Related grades by alloy family
Duplex and lean duplex
Duplex grades with about twice the yield strength of 316L: SA-240 S32304, SA-240 S32101, 1.4362 plate, SA-240 S82441, SA-240 S32003, SA-240 S32202.
Super duplex
PREN 40+ duplex grades for seawater and severe chlorides: SA-240 S32750, 1.4410 plate, 1.4501 plate, 1.4507 plate.
Same grade, other specification
Applications, forming and welding of UNS S31803
Typical uses: pressure vessels, heat exchangers, chemical tankers, FGD absorbers, desalination plant, offshore piping spools and structural members in chloride service.
Duplex sheet and plate need about 1.5–2 times the press force of 316L and show more springback. Cut by plasma, laser or waterjet and remove heat tint by pickling or grinding. For welding use a nickel-enriched duplex filler such as ER2209 (AWS A5.9), never an autogenous weld without filler. Keep the weld area clean and free of carbon-steel contamination, and pickle and passivate after welding where corrosion resistance matters.
Welding practice. Keep heat input in the range of about 0.5–2.5 kJ/mm and interpass temperature below about 150 °C. Too low a heat input gives a highly ferritic weld and HAZ; too high a heat input or slow cooling forms intermetallics. Use argon with 1–2 % nitrogen for GTAW where the specification allows, and back-purge root runs. Qualify the procedure with ferrite measurement and, where specified, A923 tests on the weld.
Certificates, testing and receiving inspection
Every delivery carries a mill certificate to ASME SA-480/SA-480M with heat analysis, tensile results and hardness, and the grade and standard as ordered. Supplementary tests we can arrange: ASTM A923 Methods A, B and C, ferrite count to ASTM E562, ASTM G48 pitting test, Charpy impact at the project temperature, and PMI on each plate. Third-party witness by SGS, BV, TÜV, DNV, ABS or LR is available with EN 10204 3.2 certificates.
On receipt, check marking and heat number against the certificate, measure thickness at several points and confirm the finish and edge condition before cutting.
Common mistakes when specifying UNS S31803
- Ordering by UNS number only, without minimum N or PREN, and receiving a heat at the bottom of the range.
- Assuming impact or ferrite requirements from one project apply to all; they come from the project specification, not the product standard.
- Using 2205 design data for a lean duplex grade, or the reverse; strength and PREN differ.
Each of these can be avoided by writing the requirement into the purchase order and checking it on the certificate before the material is cut.
Sourcing UNS S31803: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Phase balance and intermetallics | solution-anneal records checked; A923 and ferrite tests agreed before production |
| Low nitrogen at the bottom of the range | minimum N and PREN written into the order and confirmed from the heat analysis |
| Small quantities across many sizes | mixed thicknesses and grades combined in one shipment |
| Cutting and edge preparation | in-house shearing, plasma, laser and waterjet cutting, bevelling |
| Delivery delays | weekly production and shipping updates with photos |
How to order UNS S31803 plate
State the standard and edition (ASME SA-240/SA-240M), the grade (UNS S31803), thickness, width and length or coil, finish, quantity, tolerance class, any added chemistry limits, the supplementary tests and acceptance values from your specification, the certificate type and inspection agency, and packing. Send the list to SHH STEEL and we will reply with price, available stock and lead time.
FAQ
-
What is the difference between SA-240 and A240 for S31803?
- The chemistry and tensile requirements are the same. SA-240 is the ASME Code edition, so plate for pressure vessels must be certified and marked SA-240; dual-certified A240/SA-240 plate covers both.
-
Is UNS S31803 equivalent to UNS S32205?
- They are the same alloy designation in different standards. Limits are closely matched, but always order to the standard named in your specification or ask for multiple certification.
-
What ferrite range should I specify for UNS S31803?
- Use your project specification. Many specifications ask for 35–55 % ferrite measured to ASTM E562; the product standard itself does not set a range.
-
Can I order small quantities or cut sizes?
- Yes. We combine mixed thicknesses and grades into one shipment and cut plate and sheet to size in our workshop.
-
Which certificates and tests can you provide?
- Every order ships with a mill certificate (EN 10204 3.1 type) showing heat analysis and mechanical tests. Supplementary tests and 3.2 certificates with SGS, BV, TÜV or another agency are available by agreement.
Conclusion
UNS S31803 plate should be ordered with the points the standard leaves open written into the contract: finish, tolerance class, any extra chemistry limits and the supplementary tests your application needs. With those fixed, stock material from China is a fast and reliable route.