ASME SA240 UNS S32205 Stainless Steel Plate
What is ASME SA240 UNS S32205 stainless steel plate?
UNS S32205 is the standard duplex stainless steel, with 22.0–23.0 % Cr, 4.5–6.5 % Ni, 3.0–3.5 % Mo and 0.14–0.20 % N. Its austenite-ferrite structure gives about twice the yield strength of 316L, with good chloride pitting and stress-corrosion-cracking resistance. A240 lists the type name 2205 as a common name, not a trademark. Duplex stainless steels have a mixed structure of roughly equal amounts of ferrite and austenite after correct solution annealing. This gives about twice the yield strength of standard austenitic grades and much better resistance to chloride stress-corrosion cracking. Nitrogen strengthens the austenite and improves pitting resistance. Duplex plate is magnetic because of its ferrite content. For buyers, the practical point is that UNS S32205 (Type 2205) is ordered, tested and certified as SA-240 / A240 plate, so the purchase order, the mill test report and the plate marking must all show the UNS number and the specification edition.
This page sets out the SA-240 and A480 requirements for UNS S32205 (Type 2205) plate, sheet and strip: specification data, heat and product analysis limits, mechanical properties, heat treatment, the nearest EN, JIS and GB/T grades, sizes, testing and the documents that come with each shipment. SHH STEEL supplies S32205 plate mill-direct from long-term mill partners and advises buyers on grade selection, dual certification and inspection before the order is placed.
Every value on this page is taken from the specification named in each table; where a standard leaves a point to agreement, the page says so. SHH STEEL engineers can check a drawing or tender requirement against these limits before quotation.
UNS S32205 (Type 2205) specification data
UNS S32205 (Type 2205) appears in Table 1 (chemistry) and Table 2 (mechanical properties) of the specification. For ASME Code construction, order and certify to SA-240 for the Code edition named in the design; most mills issue dual ASTM A240 / ASME SA-240 certificates. Allowable stresses are not part of SA-240 and come from ASME Section II, Part D.
The table summarises how UNS S32205 (Type 2205) is specified and supplied:
| Item | Requirement / supply information |
|---|---|
| Product specification | ASME SA-240/SA-240M (ASME BPVC Section II, Part A), the Code adoption of ASTM A240/A240M |
| General requirements | ASTM A480/A480M (ASME SA-480): ordering, heat treatment, product analysis, tolerances, finish, testing, marking and certification |
| UNS designation | UNS S32205 |
| Type | Type 2205 |
| Steel family | Duplex (austenitic-ferritic) stainless steel |
| Product forms (A480 definitions) | Plate: 5.00 mm and over in thickness and over 250 mm wide. Sheet: under 5.00 mm thick and 600 mm and over wide. Strip: cold-rolled, under 5.00 mm thick and under 600 mm wide |
| Typical supply range | Hot rolled plate 3–80 mm, hot rolled coil 3–12 mm and cold rolled sheet 0.5–6 mm. |
| Width / length (typical) | 1000–2000 mm wide (wider plate by mill campaign); 2000–6000 mm long, coil, or cut to size |
| Heat-treatment condition | 1040 °C [1900 °F] minimum, then quenched in water, except that coiled product heat treated in a continuous annealing line shall be water quenched or rapidly cooled by other means (A480 Table A1.2) |
| Finish | Plate: hot-rolled, heat treated and pickled (essentially No. 1). Sheet: No. 1, 2D, 2B or bright annealed; polished No. 3 / No. 4 on request |
| Mandatory tests | Heat analysis; tension test (tensile, 0.2 % yield, elongation), hardness |
| Optional tests (when ordered) | PMI, ultrasonic testing, Charpy impact (S1), 1 % offset yield (S3), detrimental phases to A923 or A1084 |
| Dimensional tolerances | A480 Annex A2 (inch-pound) or Annex A3 (A480M, SI), by production route and product width |
| Marking | Specification, type or UNS designation, material identification (heat) number and manufacturer’s name or mark (A480 25.1) |
| Certificates | Material test report to A480 Section 8; EN 10204 3.1 as standard; EN 10204 3.2 with third-party witness on request |
Under A480 1.2, the product specification prevails over A480 when the two conflict, and a more stringent purchase-order requirement prevails over both. The purchase order cannot waive a test or relax a requirement of either specification. State the unit system (A240 or A240M) on the order.
UNS S32205 chemical composition: heat analysis and product analysis
The heat analysis limits for UNS S32205 (Type 2205) are below, in percent by mass (maximum unless a range or minimum is shown), from A240/SA-240 Table 1:
| Grade | C | Mn | P | S | Si | Cr | Ni | Mo | N |
|---|---|---|---|---|---|---|---|---|---|
| UNS S32205 | 0.030 | 2.00 | 0.030 | 0.020 | 1.00 | 22.0–23.0 | 4.5–6.5 | 3.0–3.5 | 0.14–0.20 |
Heat analysis versus product analysis. The heat (melt or ladle) analysis is made by the steel producer on a sample taken during pouring or from in-process product (A480 6.2). It must meet the Table 1 limits exactly, and it is the analysis reported on the mill test report. A product (check) analysis is an analysis of the finished plate, which the purchaser may make to verify its identity (A480 7.1). Because of segregation and sampling, it is allowed to fall slightly outside the Table 1 limits by the tolerances of A480 Table A1.1. These tolerances do not apply to the heat analysis. The comparison below applies them to S32205:
| Element | Heat (melt/ladle) analysis, % — A240/SA-240 Table 1 | Product analysis tolerance — A480/SA-480 Table A1.1 | Permitted product (check) analysis, % |
|---|---|---|---|
| Carbon (C) | 0.030 max | 0.005 over max | ≤ 0.035 |
| Manganese (Mn) | 2.00 max | 0.04 over max | ≤ 2.04 |
| Phosphorus (P) | 0.030 max | 0.005 over max | ≤ 0.035 |
| Sulfur (S) | 0.020 max | 0.005 over max | ≤ 0.025 |
| Silicon (Si) | 1.00 max | 0.05 over max | ≤ 1.05 |
| Chromium (Cr) | 22.0–23.0 | 0.25 under min / 0.25 over max | 21.75–23.25 |
| Nickel (Ni) | 4.5–6.5 | 0.10 under min / 0.10 over max | 4.40–6.60 |
| Molybdenum (Mo) | 3.0–3.5 | 0.10 under min / 0.10 over max | 2.90–3.60 |
| Nitrogen (N) | 0.14–0.20 | 0.02 under min / 0.02 over max | 0.12–0.22 |
How to read the table: the tolerance band is chosen by the specified limit, or by the maximum of a specified range, and is applied below the minimum and above the maximum. Under A480 7.2, several determinations of one element in a heat must show the same tendency; they may not fall both above and below the range. Where a requirement is a ratio, such as Ti ≥ 5×(C+N), the ratio found by product analysis must be at least 0.90× the specified minimum (A480 A1.1).
A480 6.3.1 also sets allowances for unspecified copper, molybdenum, titanium and niobium (Cu 0.75 %, Mo 0.75 %, Ti 0.10 %, Nb 0.10 %). These prevent one grade being certified when it actually meets another grade’s composition. Handheld XRF PMI confirms alloy identity but cannot measure carbon or nitrogen. When an L, H or nitrogen-controlled grade must be proven, a laboratory or spark-OES product analysis is needed.
What the main elements do in S32205:
- Carbon ≤ 0.030 %: low carbon limits chromium carbide precipitation in weld heat-affected zones.
- Chromium 22.0–23.0 %: forms the passive film that makes the steel stainless; higher chromium improves resistance to corrosion and oxidation.
- Nickel 4.5–6.5 %: balances the microstructure and improves toughness.
- Molybdenum 3.0–3.5 %: improves resistance to pitting and crevice corrosion in chloride media.
- Nitrogen 0.14–0.20 %: strengthens the steel and improves pitting resistance; in duplex grades it also helps keep the phase balance after welding.
Indicative PREN (Cr + 3.3 Mo + 16 N) calculated by SHH STEEL from the minimum Table 1 values is about 34.1. This is not a specification requirement; the PREN of a given heat is calculated from its actual analysis and is usually higher.
UNS S32205 mechanical properties (annealed)
Room-temperature tensile and hardness requirements for UNS S32205 (Type 2205) in the annealed condition (ASTM A240/A240M Table 2):
| Condition / thickness | Tensile strength, min | Yield strength 0.2 %, min | Elongation in 50 mm, min | Hardness, max | Cold bend |
|---|---|---|---|---|---|
| All thicknesses | 655 MPa [95 ksi] | 450 MPa [65 ksi] | 25 % | 293 HBW / 31 HRC | not required |
Yield strength is the 0.2 % offset value; 1 % offset yield can be reported when ordered under Supplementary Requirement S3, and Charpy impact tests under Supplementary Requirement S1.
Bend tests are not required for austenitic or duplex grades.
Tension specimens are taken from finished material and tested to ASTM A370 (A480 17.1). For cut-length plate, A480 16.1.2 requires one tension test and one or more hardness tests for each 100 pieces or fewer of the same heat and nominal thickness heat treated together; coil product is tested from each coil. Retests follow A370 and A480 Section 20.
The values in Table 2 are room-temperature minimums for acceptance. Design strength at temperature, including allowable stresses for ASME Code calculations, comes from ASME Section II, Part D and the construction code, not from SA-240.
Heat treatment of UNS S32205 plate
Heat treatment for UNS S32205 (Type 2205): 1040 °C [1900 °F] minimum, then quenched in water, except that coiled product heat treated in a continuous annealing line shall be water quenched or rapidly cooled by other means (A480 Table A1.2).
A480 15.1 requires the heat treatment to be a separate thermal cycle; in-process thermal cycles may not replace the annealing cycle. Material that fails a test may be re-heat-treated and resubmitted (A480 20.5).
For duplex grades, correct annealing temperature and fast cooling are essential to dissolve intermetallic phases and set the ferrite-austenite balance. Re-annealing after hot forming should follow the same Table A1.2 limits.
Key characteristics of UNS S32205 (Type 2205)
UNS S32205 (Type 2205) is a standard duplex stainless steel. The points that matter most when specifying it:
- Minimum tensile 655 MPa, yield 450 MPa and elongation 25 %; hardness up to 293 HBW.
- Higher Cr, Mo and N minimums than the older S31803, so S32205 plate is often dual certified S31803/S32205.
- Detrimental intermetallic phases can be checked to ASTM A923 when the order specifies it.
- Welding procedures must keep the ferrite-austenite balance.
Pitting resistance is often compared by PREN, the pitting resistance equivalent number (Cr + 3.3 Mo + 16 N). Duplex grades are generally limited to service below about 300 °C. Long exposure in the intermediate temperature range causes 475 °C embrittlement of the ferrite and, at higher temperatures, precipitation of intermetallic phases such as sigma. Correct solution annealing and rapid cooling, as fixed in A480 Table A1.2, are therefore part of the specification.
UNS S32205 equivalent grades: ASTM/ASME, EN, JIS and GB/T compared
Equivalent grades are cross-references, not interchangeable specifications. Each standard sets its own element ranges, minimum properties, test methods and product-form rules, so a plate certified to one standard is only certified to another when the same heat has been tested against both and the certificate says so. SHH STEEL checks every dual- or multi-standard request against each standard line by line before confirming the order.
| System | Standard | Designation | Closeness | What to check |
|---|---|---|---|---|
| ASME / ASTM | SA-240 / A240 with A480 / SA-480 | UNS S32205 (Type 2205) | reference grade | Specification edition required by the code or contract |
| EN | EN 10088-2 / EN 10028-7 | 1.4462 X2CrNiMoN22-5-3 | nearest equivalent; not identical | Steel number and name; proof strengths Rp0.2/Rp1.0 depend on product form (C, H or P) and thickness; elongation is measured on a different gauge length |
| JIS | JIS G4304 (hot-rolled) / G4305 (cold-rolled) | SUS329J3L | commonly cross-referenced; not identical | SUS designation; chemistry ranges set independently; check carbon, nitrogen and nickel against the A240 row |
| GB/T | GB/T 4237 (hot-rolled) / GB/T 3280 (cold-rolled) | 022Cr23Ni5Mo3N (S22053) | commonly cross-referenced; not identical | GB/T 20878 name and numeric code; the numeric code is not a UNS number even when it looks similar |
European standards. EN 10088-2 covers corrosion-resisting stainless steel sheet, plate and strip for general purposes. EN 10028-7 covers flat stainless products for pressure purposes and is the flat-product standard normally used for pressure equipment in Europe. Both use a steel number (1.4xxx) and a steel name built from the composition, and many steel numbers appear in both, but confirm that the steel number is listed in the edition you need. EN values for 0.2 % and 1 % proof strength depend on product form (cold-rolled strip C, hot-rolled strip H, hot-rolled plate P) and thickness. EN elongation is measured on proportional or 80 mm gauge lengths, so it cannot be compared directly with the A240 elongation in 50 mm.
Japanese standards. JIS G4304 covers hot-rolled and JIS G4305 cold-rolled stainless plate, sheet and strip, both with SUS designations. JIS chemistry ranges are close to the AISI-type grades but are set independently, so carbon, nitrogen and nickel limits should be checked against the A240 row whenever a heat must meet both.
Chinese standards. GB/T 4237 covers hot-rolled and GB/T 3280 cold-rolled stainless plate, sheet and strip, using GB/T 20878 grade names such as 06Cr19Ni10 and numeric codes such as S30408. The numeric code is a Chinese designation and is not a UNS number, even where the digits look similar. Always state the standard next to the code on purchase orders and certificates.
Related ASTM and ASME specifications. A240 and SA-240 share the same technical content; ASME adopts a specific A240 edition for each Code edition, so Code work should name SA-240. General requirements come from A480 / SA-480. Clad plate with this cladding is ordered to A264 (Cr-Ni steel-clad plate). Other product forms use their own specifications (pipe, forgings, bar), so check that the UNS number is listed in each one before ordering a matching set.
In practice, SHH STEEL offers dual-certified plate (for example A240 / EN 10088-2) when a mill heat is designed to meet both standards. When it cannot be, we recommend ordering to the single standard the design code requires and treating the others as reference only.
UNS S32205 (Type 2205) compared with related grades
Grades buyers most often compare with UNS S32205 (Type 2205):
- ASME SA240 UNS S32304 stainless steel plate — UNS S32304 (Type 2304): C ≤ 0.030 %, Cr 21.5–24.5 %, Ni 3.0–5.5 %, Mo 0.05–0.60 %, N 0.05–0.20 %; minimum yield 400 MPa
- ASME SA240 UNS S32750 stainless steel plate — UNS S32750 (Type 2507): C ≤ 0.030 %, Cr 24.0–26.0 %, Ni 6.0–8.0 %, Mo 3.0–5.0 %, N 0.24–0.32 %, Cr + 3.3 Mo + 16 N ≥ 41; minimum yield 550 MPa
- ASME SA240 UNS S32101 stainless steel plate — UNS S32101: C ≤ 0.040 %, Cr 21.0–22.0 %, Ni 1.35–1.70 %, Mo 0.10–0.80 %, N 0.20–0.25 %; minimum yield 450 MPa
The site also has pages organised by type designation for the same or closely related material: ASTM A240 Type 2205 stainless steel sheet & plate, ASME SA240 2205 stainless steel plate. This page is the UNS-number reference for SA-240 orders; the material is the same where the grade is the same.
All grades in this series are listed under ASME SA240/SA240M stainless steel plate and ASTM A240/A240M stainless steel plate.
Applications of SA240 UNS S32205 plate
Typical uses of UNS S32205 (Type 2205) plate, sheet and strip:
- Oil and gas process vessels and separators
- Chemical tankers and storage tanks
- Heat exchangers and desalination equipment
- Pulp and paper digesters and structural parts
The final choice should always be checked against the service medium, temperature and design code; SHH STEEL can share mill corrosion data and reference projects on request.
Designers choose duplex grades where higher strength can reduce thickness and weight, or where chloride stress-corrosion cracking rules out austenitic grades. Lean duplex grades compete with 304L/316L, standard duplex with 316L and 317L, and super duplex with high-alloy austenitic and nickel-base materials. Fabrication needs qualified welding procedures and, when specified, phase testing to ASTM A923 or A1084.
UNS S32205 (Type 2205) sizes, finishes and supply forms
Size ranges below are typical mill capabilities for UNS S32205 (Type 2205), not limits set by the specification; actual availability depends on the mill campaign and is confirmed at quotation.
| Item | Typical supply range |
|---|---|
| Product forms | Hot rolled plate 3–80 mm, hot rolled coil 3–12 mm and cold rolled sheet 0.5–6 mm. |
| Width | 1000, 1219, 1250, 1500, 1800, 2000 mm; wider plate by mill |
| Length | 2000, 2438, 3000, 6000 mm, coil, or cut to size |
| Surface finish | No.1 (hot rolled, heat treated and pickled) for plate; 2B or 2D for cold rolled sheet |
| Tolerances | ASTM A480/A480M, or tighter by agreement |
For weight estimates, plate weight (kg) ≈ thickness (mm) × width (m) × length (m) × density, with density about 7.8 g/cm³ for this grade family. The mill certificate weight governs invoicing.
Plate finishes under A480 Section 13 range from heat treated with scale left on, which is used for heat-resisting service because scale impairs corrosion resistance, to blast-cleaned or pickled, which is essentially a No. 1 finish and the usual choice for corrosion service. Sheet finishes under Section 11 include No. 1, 2D (dull, good for deep drawing), 2B (smooth, moderately reflective), bright annealed, and polished No. 3, 4, 6, 7 and 8. Thickness should be ordered as a decimal or fractional dimension, not a gauge number (A480 4.1.7).
Forming, welding and heat treatment of UNS S32205
Duplex plate needs higher forming forces than austenitic plate because of its higher yield strength; allow for more springback.
Weld with duplex fillers (usually over-alloyed in nickel) and qualified heat-input limits, so the weld and heat-affected zone keep a balanced ferrite-austenite structure.
Avoid long exposure in the intermediate temperature range where intermetallic phases form; any solution annealing and cooling must follow ASTM A480/A480M.
Repair of plate surface defects by welding is permitted unless prohibited by other specifications or the order (A480 Section 21). Defect depth may not exceed one-third of nominal thickness, and the total repaired area may not exceed 1 % of the plate surface, without the purchaser’s prior approval. Welding procedures and welders must be qualified to ASME Section IX, consumables must suit the plate, and the repaired area must be ground smooth. Buyers who do not accept weld repairs should say so on the order.
Cutting is normally by plasma, waterjet or abrasive saw; avoid oxy-fuel cutting on stainless steel. Keep stainless plate away from carbon-steel dust and tools during handling and fabrication, because embedded iron causes rust staining. Pickling and passivation after fabrication restore the passive surface.
Testing, inspection and certificates for S32205 plate
Each heat is tested to SA-240 / A240 and ASTM A480/A480M: heat analysis, tension tests and hardness, plus the surface and dimensional checks for the product form.
Mill test certificates to EN 10204 3.1 are standard. EN 10204 3.2 certificates with third-party witness (TUV, ABS, CCS, BV, DNV, LR or an inspector named by the buyer) can be arranged, together with optional tests such as PMI, intergranular corrosion, ultrasonic testing and Charpy impact (Supplementary Requirement S1), and detrimental-phase testing to ASTM A923 or A1084.
Tests for detrimental intermetallic phases (Methods A, B or C of A923, or A1084 for lean duplex) are not required unless specified, but all duplex types listed in those methods are expected to pass (A480 18.3).
Plate is marked in two places near the ends, or line-marked along one edge, with the specification, type or UNS number, heat number and manufacturer; material under 6.4 mm is not die-stamped (A480 25.1). The supplier must pass on a copy of the original mill test report (A480 8.4), and test-based rejections must be reported within 60 working days of receipt (A480 23.1).
Common buyer concerns and SHH STEEL solutions
The concerns below come up most often when buyers source UNS S32205 (Type 2205) plate from China, together with how SHH STEEL deals with each one.
| Buyer Concern | SHH STEEL Solution |
|---|---|
| Fake material or certificates | Each heat can be checked by TUV, ABS, CCS or another class society as third-party witness, and partner laboratories run PMI, chemical and mechanical tests against the order. Third-party witness and EN 10204 3.2 certificates available. |
| Unsafe deposit | TT and LC are both accepted, including TT + LC combinations. For large projects the buyer can sign directly with the mill, and SHH STEEL handles coordination and documents for a small service fee. |
| Small orders below mill MOQ | Small quantities are consolidated with other customers’ orders of the same grade and thickness, so even lots below the mill MOQ are rolled as genuine mill production with full traceability. |
| Slow delivery | Dedicated staff chase the mill delivery schedule and report progress at melting, rolling, heat treatment, testing and packing, so delays are seen early. |
| Processing needs | Our own workshop provides cutting, bevelling, machining to drawings and surface pretreatment as value-added services, so plates arrive ready for fabrication. |
How to order UNS S32205 plate from SHH STEEL
A480 4.1 makes the purchaser responsible for stating every requirement. A complete enquiry for S32205 plate should include:
- Quantity (weight and number of pieces).
- Specification and edition: ASME SA-240 or ASTM A240 (with edition) and A480; add “M” for SI units.
- Type or UNS designation: UNS S32205 (Type 2205).
- Condition (hot-rolled or cold-rolled, annealed or heat treated) and finish; for polished finishes, one or both sides.
- Form (plate, sheet or strip) and dimensions (thickness, width and length, in the same units).
- Supplementary requirements and special tests (Charpy, intergranular corrosion, phase tests, UT, PMI).
- Inspection document (EN 10204 3.1 or 3.2), third-party inspector, marking and packing requirements.
SHH STEEL works as a sourcing and supply partner with long-term mill relationships. We help select the grade, check dual-certification options, consolidate small lots, follow production at the mill and process plates in our own workshop before shipment. Payment by TT or LC is accepted.
For S32205, the SHH STEEL team can also share recent mill test reports for reference, confirm which thicknesses are in the current rolling campaign and propose a cutting plan that reduces scrap. Send your enquiry with drawings or a cutting list and we will reply with a quotation, lead time and inspection plan.
FAQ
-
What is the difference between S32205 and S31803?
- Both are 22Cr duplex grades, but S32205 has higher minimums for chromium (22.0 %), molybdenum (3.0 %) and nitrogen (0.14 %), which give more consistent corrosion resistance. Many mills certify plate to both.
-
Is SA240 S32205 magnetic?
- Yes. Duplex steels contain roughly half ferrite, so they are magnetic; this is normal and not a sign of wrong material.
-
Do I need an A923 test for duplex plate?
- A240 does not require it unless the order says so, but many project specifications do. State ASTM A923 Method A, B or C on the purchase order if you need it.
-
Where can I buy ASME SA240 UNS S32205 plate in small quantities?
- SHH STEEL consolidates small orders of S32205 with other customers’ orders of the same grade, so lots below the mill MOQ can still be placed against mill production. Cut-to-size pieces can be supplied from our workshop.
-
What certificates come with S32205 stainless steel plate?
- Plates are supplied with EN 10204 3.1 mill test certificates to SA-240 / A240. Third-party witness and EN 10204 3.2 certificates available, issued with TUV, ABS, CCS or another nominated inspector.
-
What is the lead time for S32205 plate from China?
- Lead time depends on the mill rolling schedule, thickness and the tests ordered, and is confirmed with the quotation. Dedicated SHH STEEL staff follow the mill schedule and report progress until shipment.
Conclusion
ASME SA240 UNS S32205 Stainless Steel Plate is ordered as UNS S32205 (Type 2205), a standard duplex stainless steel. Specify the standard and edition, the UNS number, the inspection document and any supplementary tests on the order so the certificate can be checked line by line. SHH STEEL supports the order from grade check to delivery, and you can contact SHH STEEL for a quotation, mill-direct supply and processing to your drawings.