ABS EH40 Shipbuilding Steel Plate Supplier
What is ABS EH40 shipbuilding steel plate?
Equivalent grades: ABS EH40 ≈ ASTM A131 Grade EH40 ≈ DNV NV E40 ≈ LR EH40 ≈ BV EH40 ≈ CCS E40 / EH40 ≈ NK KE40 ≈ KR RE40 ≈ RINA EH40 ≈ GB 712 Grade EH40 (all class-approved, stamped by the issuing society).
ABS EH40 is a higher-strength hull structural steel under ABS Rules Part 2, Chapter 1, Section 3 (2-1-3). It belongs to the E-class (−40 °C) toughness group at strength level 40: minimum yield 390 N/mm², tensile 510–650 N/mm², elongation 20 % min. Plates are die-stamped AB/EH40 after ABS survey. EH40 is the −40 °C higher-strength grade at 390 N/mm² yield; plate is typically N/TM with each-piece impact in many Table 5 cells.
Thickness coverage for plates: AH/DH/EH 32/36 and AH/DH/EH 40 / FH 32/36/40 are listed up to 150 mm (2-1-3/1). Ordinary-strength ABS Grade A / ABS B / ABS D / ABS E stay at 235 N/mm² yield; EH40 is selected when scantlings need the higher yield of the 40 band.
SHH STEEL supplies ABS EH40 from ABS-approved Chinese mills, stock or mill roll, with optional multi-class and EN 10204 3.2. Related pages: ABS EH32 / ABS EH36; same strength other toughness: ABS AH40 / ABS DH40 / ABS FH40.
Buyer note for EH40: EH plate routes in Table 5 are dominated by N/TM with each-piece impact — plan mill time like ordinary Grade E, not like AH stock. Live reference for ordinary strength: ABS Grade A.
ABS EH40 plate: specification summary
| Item | ABS EH40 data |
|---|---|
| Rule | ABS Rules Part 2, 2-1-3 Higher-strength Hull Structural Steel (2023 checked); general 2-1-2 clauses also apply |
| Strength level | higher strength 40, yield 390 N/mm² min., tensile 510–650 N/mm² |
| Toughness class | EH → Charpy at −40 °C |
| Plate thickness covered | up to and including 150 mm (as listed for this grade family in 2-1-3/1) |
| Deoxidation | killed, fine grain practice (2-1-3/5) |
| Impact test | Charpy V at −40 °C; frequency and supply condition per 2-1-3/7.3 Table 5 |
| Marking | AB/EH40 (+ Z/U if ordered) |
| TMCP Ceq (Table 6) | ≤ 0.40 % for t ≤ 50 mm; ≤ 0.42 % for 50 < t ≤ 100 mm (TM steels) |
| Thickness tolerance | minus 0.3 mm (2-1-1/15.3) |
| Certificate | ABS Surveyor-endorsed mill certificate; EN 10204 3.1 / 3.2 on request |
Size range. Common market thicknesses for EH40 are about 6–80 mm (heavier plates available as per mill approval), widths 1500–3500 mm. Exact maximum thickness for a given delivery condition is as per standard and mill certificate / ABS works approval.
ABS EH40 chemical composition (heat and product analysis)
| Element | Heat (ladle) analysis, % | Product (check) analysis, % | Note |
|---|---|---|---|
| C | 0.18 max. | 0.22 max. (0.18 + 0.04) | AH/DH/EH group |
| Mn | 0.90–1.60 (AH ≤12.5 mm may be 0.70 min.) | 0.81–1.72 (0.90 − 0.09; 1.60 + 0.12) | Note 3: AH ≤12.5 mm may use 0.70 % Mn min. |
| Si | 0.10–0.50 | 0.04–0.56 (0.10 − 0.06; 0.50 + 0.06) | min. waived if acid-soluble Al ≥ 0.015 % |
| P | 0.035 max. | 0.045 max. (0.035 + 0.010) | |
| S | 0.035 max. | 0.045 max. (0.035 + 0.010) | |
| Al (acid soluble) min. | 0.015 min. acid-soluble (or total Al per 2-1-3/5) | 0.015 min. (Al not listed in ASTM A6/A6M Table A – heat limit applies) | or total Al per 2-1-3/5; grain refining |
| Nb | 0.02–0.05 when used singly | 0.01–0.06 (0.02 − 0.01; 0.05 + 0.01) | when used singly; combined minima in 2-1-3/5 |
| V | 0.05–0.10 when used singly | 0.04–0.11 (0.05 − 0.01; 0.10 + 0.01) | when used singly |
| Ti | 0.02 max. | 0.03 max. (0.02 + 0.01) | need not be reported unless intentionally added |
| Cu | 0.35 max. | 0.38 max. (0.35 + 0.03) | may report ≤ 0.02 % if below |
| Cr | 0.20 max. | 0.24 max. (0.20 + 0.04) | |
| Ni | 0.40 max. | 0.43 max. (0.40 + 0.03) | FH allows higher Ni than AH/DH/EH |
| Mo | 0.08 max. | 0.09 max. (0.08 + 0.01) | |
| N | — | no heat limit specified – report actual value | not specified as a max in AH/DH/EH Table 1 |
Product (check) analysis column = heat (ladle) limit adjusted by ASTM A6/A6M-19 Table A “Permitted Variations in Product Analysis”, as required by ABS Rules Part 2, 2-1-2/5.3 (maximum + “over”, minimum − “under”; row chosen by the specified upper limit); arithmetic shown in brackets.
Source: ABS 2-1-3/7.3 Table 1. Heat (ladle) analysis must meet the table. Product (check) analysis, when required, follows ABS 2-1-2/5.3 → ASTM A6 (or other national) tolerances — ABS itself publishes no numeric product limits. AH/DH/EH share one chemistry column; toughness is differentiated by impact temperature and Table 5 supply routes, not by C/Mn caps. TMCP steels must also meet Table 6 Ceq. Ask for product analysis and Ceq/Pcm on the certificate at enquiry.
ABS EH40 tensile properties
| Property | Requirement |
|---|---|
| Tensile strength | 510–650 N/mm² |
| Yield point | 390 N/mm² min. |
| Elongation | 20 % min. (alt. A flat / C round) |
Source: 2-1-3/7.3 Table 2. Alternative B specimen elongations (Table 3) for XH40:
| Thickness (mm) | ≤5 | 5–10 | 10–15 | 15–20 | 20–25 | 25–30 | 30–40 | 40–50 |
|---|---|---|---|---|---|---|---|---|
| Elongation min. % | 12 | 14 | 15 | 16 | 17 | 18 | 19 | 20 |
Same tensile band applies to AH/DH/EH/FH 40; only impact temperature and chemistry group (FH vs AH/DH/EH) change across the letter.
ABS EH40: Charpy at −40 °C and supply condition
| Thickness | Long. avg. at −40 °C | Trans. avg. at −40 °C |
|---|---|---|
| t ≤ 50 mm | 39 J | 26 J |
| 50 < t ≤ 70 mm | 46 J | 31 J |
| 70 < t ≤ 100 mm | 55 J | 37 J |
| 100 < t ≤ 150 mm | 58 J | 39 J |
Source: 2-1-3/7.3 Table 4 (full-size; either direction acceptable). Condition of supply and impact lot size follow Table 5 and depend on grain-refining element (Nb, V, Al, Al+Ti) and thickness. In brief for plates: AH grades allow “any” condition in thinner bands with 50 t lots; DH often N/TM/CR; EH/FH plate routes are predominantly N/TM with each-piece (P) impact in many cells. Exact route for your thickness is as per standard and mill certificate — state the required delivery condition on the PO.
TMCP EH40: carbon equivalent caps 0.40 % (t ≤ 50) and 0.42 % (50 < t ≤ 100) per Table 6; over 100 mm Ceq agreed with ABS at mill qualification.
Thickness tolerance and surface condition
Minus tolerance 0.3 mm (2-1-1/15.3.2). Plus/flatness/width/length per ASTM A6 or as agreed. Surface repair per 2-1-1/3; state primer/surface class in the order if needed.
ABS EH40 plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Condition | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1800 / 2000 | 6000 / 8000 | N / TM / CR | 100+ t | China |
| 8 | 1800 / 2000 | 8000 / 12000 | N / TM / CR | 200+ t | China |
| 10 | 2000 / 2200 | 8000 / 12000 | N / TM / CR | 200+ t | China |
| 12 | 2000 / 2200 / 2500 | 12000 | N / TM / CR | 200+ t | China |
| 14 | 2000 / 2200 | 12000 | N / TM / CR | 100+ t | China |
| 16 | 2000 / 2500 | 12000 | N / TM / CR | 200+ t | China |
| 20 | 2000 / 2500 | 12000 | N / TM / CR | 100+ t | China |
| 25 | 2200 / 2500 | 12000 | N / TM / CR | 100+ t | China |
| 30 | 2200 | 10000 / 12000 | N / TM / CR | 100+ t | China |
| 40 | 2200 | 10000 | N / TM / CR | 50+ t | China |
| 50 | 2200 | 8000 / 10000 | N / TM / CR | 50+ t | China |
Quantities are approximate and change daily; all stock plates carry AB/EH40 marking and ABS-endorsed mill certificates. Sizes outside the table are produced in the next mill rolling cycle, typically 3–6 weeks including ABS survey (as per standard and mill certificate for exact lead time). Send your size list and we will reply with stock vs roll.
Packing. Plates are bundled by size with steel strapping, marked with heat number, grade and ABS stamp, and shipped in containers (up to about 11.8 m) or break bulk for longer plates.
ABS EH40 equivalents
| Standard / society | Designation | Comment |
|---|---|---|
| ASTM A131/A131M | ASTM A131/A131M Grade EH40 | A131 lists AH–FH 32/36/40; product standard only |
| IACS societies | Grade EH40 | DNV/LR/BV/CCS/NK/KR/RINA unified UR W11; BV FH36 / BV FH40 |
| GB 712 | GB 712 Grade EH40 | not class approval by itself |
| Ordinary-strength ABS | ABS Grade A / Grades B, D, E | 235 N/mm² yield family |
| Same toughness other strength | ABS EH32 / ABS EH36 | EH family |
| Same strength other toughness | ABS AH40 / ABS DH40 / ABS FH40 | 40 band |
Comparisons, not substitutions. Multi-class stamps require joint survey before rolling.
ABS EH40 vs other ABS hull grades
Pick EH40 when the drawing specifies higher-strength grade EH40 (or the society equivalent). Do not substitute ordinary Grade E unless the designer recalculates scantlings — yield differs (390 vs 235). Within the 40 band, letter choice is toughness: AH 0 °C → DH −20 °C → EH −40 °C → FH −60 °C. Within the EH letter, strength steps 32 → 36 → 40 raise yield from 315 to 355 to 390 N/mm².
For yields above 390 N/mm² ABS moves to Extra High Strength (2-1-8, AQ43/DQ47…), commercially often titled AH42/AH46 — see ABS AH42 and siblings.
When ABS EH40 is the right choice: typical uses are special and primary category members, crack-arrest strakes, and hull structure for cold-route or ice-strengthened vessels needing −40 °C toughness. The Charpy temperature (−40 °C) is fixed by the letter, and the strength by the number (ReH 390 N/mm²). Pick the strength from the scantling calculation and the letter from the material class and design temperature on the approved drawing. Swapping to a different letter or strength needs class approval of the drawing change, not just a new purchase order.
Applications and welding notes for ABS EH40
Typical uses: primary hull members at −40 °C with 390 N/mm² yield; Arctic-capable merchant tonnage. See offshore platform steel plates when primary offshore grades apply.
Welding: higher-strength hull steels need approved higher-strength consumables matched to required weld-metal toughness; preheat and heat input follow the approved WPS and often track Ceq/Pcm from the mill certificate (as per standard and mill certificate). TMCP EH40 must respect Table 6 Ceq caps. Cutting by oxy-fuel/plasma/laser is routine; thick QT/FH plate may need hydrogen control — follow mill recommendations.
Within the EH letter, moving 40 → other strengths (ABS EH32, ABS EH36) changes yield/tensile/elongation and Table 4 energies, not the Charpy temperature (−40 °C). Pick strength from the scantling; pick letter from the design temperature.
Processing notes for ABS EH40: cold forming of EH40 is routine within normal shipyard radii. Line heating and fairing of TMCP plate should stay within the temperature limits recommended by the mill, because overheating can reduce the strength gained in controlled rolling. Check the delivery condition on the certificate before planning hot forming.
Certificates, ABS survey and third-party inspection
ABS survey at the mill; certificate includes ladle chemistry, Ceq where applicable, tensile, Charpy at −40 °C, delivery condition and plate identity. Optional EN 10204 3.2, UT (U), Z-direction, multi-class. On receipt: verify AB/EH40 stamp, −40 °C impact data, energies ≥ Table 4, thickness ≥ nominal − 0.3 mm.
Charpy acceptance for ABS EH40 by thickness (from 2-1-3; actual results as per standard and mill certificate):
| Thickness t (mm) | Test temperature | Average energy, longitudinal (J min.) | Average energy, transverse (J min.) |
|---|---|---|---|
| t ≤ 50 | −40 °C | 39 | 26 |
| 50 < t ≤ 70 | −40 °C | 46 | 31 |
| 70 < t ≤ 100 | −40 °C | 55 | 37 |
| 100 < t ≤ 150 | −40 °C | 58 | 39 |
On receipt, check that the test temperature on the certificate is −40 °C and that the energy matches the band for the delivered thickness, not the thinnest band. Also check that the plate number on the stamp matches the certificate line, and that the ABS Surveyor endorsement is present. If UT was ordered (e.g. EN 10160 or ASTM A578 level), check the UT report as well. If the PO asked for 3.2, the inspector’s report must name the witnessed tests and plate numbers.
Common mistakes ordering ABS EH40
- Ordering “ABS 40” without the letter (AH/DH/EH/FH) — toughness class missing
- Accepting ordinary-strength Grade E certificates for a EH40 PO
- Ignoring TMCP Ceq caps (0.40/0.42) on TM plate
- FH chemistry (tighter P/S, N) not checked when the PO says FH
- Coil-cut plate without coil approval
- Missing ABS endorsement on the MTC
- Stock vs mill roll for ABS EH40?: Common 8–25 mm EH40 is often available from China stock with EH40 marking; thicker or QT/FH routes are usually mill-roll with ABS survey (about 3–6 weeks as a commercial estimate — confirm per order).
Write grade, delivery condition, impact temperature and certificate type into the PO.
Sourcing ABS EH40: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Fake class plate | ABS-approved mills only; traceable stamp + certificate; 3.2 on request |
| Payment risk | T/T or L/C; inspection before balance |
| Mixed sizes / grades | EH40 combined with A/B/D/E or other AH–FH sizes in one container |
| Lead time visibility | weekly photo updates from dedicated coordinator |
| Prep before ship | cutting, bevelling, drilling, machining in our workshop |
How to order ABS EH40 plate
Specify ABS EH40 (2-1-3), delivery condition (AR/CR/N/TM/QT as applicable), thickness × width × length × qty, Z/U, multi-class, certificate type, port. Send to SHH STEEL.
Sample PO line: “Steel plate to ABS Rules Part 2 2-1-3, Grade EH40, delivery condition [AR/CR/N/TM/QT], 20 × 2500 × 12000 mm, 30 pcs, marked AB/EH40, certificate endorsed by ABS Surveyor, EN 10204 3.2 [if required], UT [if required], CIF [port].” Each bracketed item changes price, lead time and which mills can supply, so fix them at enquiry stage.
FAQ
Conclusion
ABS EH40 is higher-strength hull steel: yield 390 N/mm², tensile 510–650 N/mm², Charpy at −40 °C, marking AB/EH40. Lock on the order: delivery condition per Table 5, impact lot size, TMCP Ceq if TM, product analysis if needed, multi-class and 3.2.
SHH STEEL supplies EH40 from ABS-approved mills with Surveyor-endorsed certificates, stock or roll, optional 3.2 and multi-class.
T/T or L/C with inspection before balance; mixed containers; photo follow-up; in-house cutting/bevelling/drilling/machining.
Request a quotation: send SHH STEEL ABS EH40, sizes, qty, port and any multi-class/Z/U/3.2 needs.