Close view of ASTM A131 EH40 hull structural steel plate, ASTM A131/A131M

ASTM A131 EH40 Shipbuilding Steel Plate

ASTM A131 EH40 higher-strength hull plate to ASTM A131/A131M (A6/A6M general requirements): yield 390 MPa [57 ksi], impact −40 °C [−40 °F]. Mill test report, ABS or other class certificate on request — SHH STEEL.
Keywords
ASTM A131 EH40 steel plate, A131 EH40 shipbuilding steel, A131/A131M EH40 hull plate, ASTM A131 EH40 ship plate, higher-strength marine steel plate
Equivalent Grades:
ABS EH40; DNV VL E40; LR EH40; BV EH40; CCS EH40; KR RE40; NK KE40; RINA EH40; GB 712 EH40; IACS UR W11 EH40
Share:
Overview
Specification
Chemical Composition
Mechanical Properties
Impact Test and Condition of Supply
A6/A6M General Requirements
Relation to ABS Rules
Equivalent Grades
Grade Selection
Welding and Fabrication
Mill Test Report and Marking
Stock and Supply
Specification Mistakes
How to Order
FAQ
Conclusion

ASTM A131 EH40 shipbuilding steel plate — overview

Technical Reviewer: Jack | SHH STEEL Material Solutions Department · Updated: 2026-10-27

ASTM A131 EH40 is the −40 °C [−40 °F] higher-strength grade at the 40 level and the A131 plate most often called up for crack-arrest strakes: 390 MPa [57 ksi] minimum yield, 510–650 MPa [74–94 ksi] tensile, killed and fine-grain treated steel.

Equivalent grades: ABS EH40 · DNV NV E40 · LR EH40 · BV EH40 · CCS E40 / EH40 · NK KE40 · KR RE40 · RINA EH40 · GB 712 Grade EH40.

The letter sets toughness, the number sets strength: EH40 is letter E at level 40. AH40, DH40, EH40 and FH40 share tensile values and differ in impact temperature (and, for FH, chemistry).

ASTM A131/A131M is a product specification: it tells a mill what to make and test, while the general rules for plate — dimensions, tolerances, test methods, retests, marking and test reports — come from ASTM A6/A6M, which A131 references. Read the two together; neither is complete alone.

A131 was developed to mirror the American Bureau of Shipping material rules, which is why its grade letters match the IACS system. The important difference is legal, not metallurgical: an A131 plate is certified by the mill; a classed plate is additionally certified by a surveyor. US Coast Guard plan reviewers and many US owners accept A131 for non-classed or domestic work, while classed hulls normally require the society certificate (confirm with the approving authority).

SHH STEEL supplies ASTM A131 EH40 with the mill test report, ABS or other class certification on the same heat when ordered, and cutting to drawing. The full range is under ASTM A131 Grade EH40.

Where EH40 sits. EH is the crack-arrest and cold-service letter; its impact test runs at −40 °C [−40 °F]. Level 40 (390 MPa [57 ksi]) is the top of A131. It appears in heavily loaded decks, hatch coamings and offshore structure where level-36 plate would become uneconomically thick. EH is where owners, flag administrations and the classification plan most often insist on per-plate testing and full traceability.

ASTM A131 EH40: key data at a glance

ItemASTM A131 EH40
SpecificationASTM A131/A131M (structural steel for ships), higher-strength EH40 — edition to be stated on the order
General requirementsASTM A6/A6M (dimensions, tolerances, testing, marking, test reports)
Yield strength, min.390 MPa [57 ksi]
Tensile strength510–650 MPa [74–94 ksi]
Elongation, min.19 % in 200 mm [8 in.] / 22 % in 50 mm [2 in.] (UNCERTAIN — verify edition)
Charpy V-notch−40 °C [−40 °F]
Deoxidationkilled, fine-grain practice (Al, Nb, V or Ti)
Condition of supplyCR, N or TMCP within thickness limits; as-rolled only in thin gauges
Usual plate rangeabout 5–100 mm [3/16–4 in.] thick; shapes and bars are also within A131 scope
Certificationmill test report per A6/A6M; class certificate or third-party witness on request

Dual units are deliberate: A131 is written in inch-pound units and A131M in SI. The two are not exact conversions of each other, so the order must name one system as governing — mixing them on a mill order is the classic source of a borderline rejection.

For EH40 the lines that matter are the impact temperature (−40 °C [−40 °F]) and the condition of supply, which drives test frequency and the carbon-equivalent expectation.

ASTM A131 EH40 chemical composition — every element on the report

ElementHeat analysis, %Product (check) analysis, %Note
C0.18 max.0.22 max. (0.18 + 0.04)A/D/E column
Si0.10–0.500.04–0.56 (0.10 − 0.06; 0.50 + 0.06)
Mn0.90–1.60 (0.70 min. permitted for AH ≤ 12.5 mm)0.81–1.72 (0.90 − 0.09; 1.60 + 0.12)
P0.035 max.0.045 max. (0.035 + 0.010)
S0.035 max.0.045 max. (0.035 + 0.010)
Al (acid-soluble)0.015 min. acid-soluble (or 0.020 min. total)0.015 min. (Al not listed in ASTM A6/A6M Table A – heat limit applies)grain refiner
Nb0.02–0.050.01–0.06 (0.02 − 0.01; 0.05 + 0.01)grain refiner / strength
V0.05–0.100.04–0.11 (0.05 − 0.01; 0.10 + 0.01)
Ti0.02 max.0.03 max. (0.02 + 0.01)
Cu0.35 max.0.38 max. (0.35 + 0.03)
Cr0.20 max.0.24 max. (0.20 + 0.04)
Ni0.40 max.0.43 max. (0.40 + 0.03)
Mo0.08 max.0.09 max. (0.08 + 0.01)
Nnot specified (report on request)no heat limit specified – report actual value
Nb+V+Ti0.12 max. (combined, when used together)not applicable (calculated from heat analysis)combined microalloy cap
Ceq (TMCP plate)0.40 / 0.42 max. (calculated)not applicable (calculated from heat analysis)≤ 50 / 50–100 mm, when TMCP

Product (check) analysis column = heat (ladle) limit adjusted by ASTM A6/A6M-19 Table A “Permitted Variations in Product Analysis”, which ASTM A131/A131M invokes through A6/A6M (maximum + “over”, minimum − “under”; row chosen by the specified upper limit); arithmetic shown in brackets.

Values follow the IACS UR W11 / ABS basis that A131 tracks; the A131 table in the edition named on your order governs (no local copy checked — UNCERTAIN). For EH40, mills typically rely on Nb–Ti microalloying, low sulphur and calcium treatment to secure −40 °C in thick plate.

US mill test reports print a fixed analysis list — commonly C, Mn, P, S, Si, Cu, Ni, Cr, Mo, V, Nb, Al and sometimes Ti, N, B and Ca — regardless of grade. That makes residual-element screening easy: compare every line, not only the ones A131 limits.

A131 requires the heat analysis to be reported for every element with a limit in its table; where a grade allows grain-refining elements, the one actually used must be shown so the inspector can confirm fine-grain practice. Residuals that A6/A6M asks to be reported (Cu, Ni, Cr, Mo, V, Nb) normally appear even when A131 itself sets no limit (confirm A6/A6M reporting rule for the cited edition).

ASTM A131 EH40 tensile requirements

PropertySI (A131M)Inch-pound (A131)
Yield strength, min.390 MPa57 ksi
Tensile strength510–650 MPa74–94 ksi
Elongation in 200 mm [8 in.], min.19 %same
Elongation in 50 mm [2 in.], min.22 %same

A131 follows A6/A6M practice for specimens: rectangular 200 mm [8 in.] or 50 mm [2 in.] gauge specimens, or round specimens in heavy plate, with elongation minimums tied to the gauge length — not the proportional 5.65√S₀ gauge used in European and class certificates. That is why the elongation figure on an A131 report can look lower than on a class certificate for the same steel (gauge-length adjustments for thin/thick plate per A6/A6M — UNCERTAIN).

AH40, DH40, EH40 and FH40 share these tensile values. Against Grade A the yield gain is 155 MPa, which the designer converts into thinner plate.

A131 reports tensile results in both unit systems when the order is written to A131M or to the dual standard; the order must say which system governs, because rounding is not identical. For TMCP higher-strength plate the yield/tensile ratio is often 0.80–0.90; A131 sets no ratio limit, so add one as a supplementary requirement if your design code needs it (indicative).

ASTM A131 EH40: Charpy V-notch at −40 °C [−40 °F] and condition of supply

EH plate is N or TMCP and tested more frequently than AH or DH — often per plate.

ThicknessAvg. longitudinal (J)Avg. transverse (J)
≤ 50 mm [2 in.]3926
50–70 mm4631
70–100 mm5537

Each value is the average of three full-size specimens; one may fall below the average but not below 70 % of it. Longitudinal specimens apply unless transverse are ordered. Impact testing itself is done to ASTM A370 / E23 practice referenced through A6/A6M (clause numbers not quoted — UNCERTAIN).

The test lot rule is where A131 and the society rules are most often confused on the shop floor: the report should state the condition of supply, because it decides whether one set of three covers a batch, a plate-as-rolled or each heat-treated plate.

How ASTM A6/A6M governs ASTM A131 EH40

Almost everything a receiving inspector checks on ASTM A131 EH40 apart from chemistry and mechanical values comes from A6/A6M: thickness, width, length and flatness tolerances; camber; permissible variations in weight; surface-imperfection removal by grinding; weld repair limits; retest rules; and the content of the test report.

Thickness tolerance is the point to watch. Class rules apply a small fixed minus tolerance to hull plate (IACS UR W13, commonly −0.3 mm), while A6/A6M expresses plate tolerances as variations over ordered thickness and weight (table numbers not quoted — UNCERTAIN). For classed hulls state on the order that the class minus tolerance applies; for domestic A131 work, A6/A6M governs.

Supplementary requirements in A6/A6M — for example ultrasonic examination (to A435 or A578), product analysis, through-thickness testing or additional tension tests — apply only when ordered by number. If it is not on the purchase order, the mill is not obliged to do it.

Heat vs. plate-as-rolled. A6/A6M distinguishes the heat (the melt) from the plate-as-rolled (the product of one slab or ingot). Test frequencies in A131 are expressed against those units, so a report listing one heat but several plates-as-rolled should show results for each unit the standard requires.

ASTM A131 EH40 and the ABS Rules for Materials and Welding

A131 and the ABS Rules (Part 2) share grade letters, chemistry columns and test values because A131 was written to align with them. A plate certified only to A131 is, however, not an ABS plate: ABS certification requires an ABS-approved mill, survey of testing and the ABS stamp on the plate.

In practice US and Gulf Coast yards order “ASTM A131 EH40 / ABS EH40” dual-certified material. The mill makes one heat, the surveyor witnesses or audits the tests, and the plate is stencilled with both. Where a vessel is not classed — many inland barges and domestic workboats — A131 alone is often what the owner and the approving authority require.

Edition mismatches happen: the ABS Rules are revised yearly, while the A131 year is fixed on the order. If the contract cites both, state which governs in case of difference.

ASTM A131 EH40 against classification-society grades

Standard / societyDesignationRemark
ASTM A131/A131M (this page)ASTM A131 EH40US product specification; general requirements in A6/A6M
ABSABS EH40Rules Part 2 — the reference A131 was written to mirror
DNVDNV VL E40VL prefix
LRLR EH40
BVBV EH40
CCSCCS EH40
KRKR RE40R-prefix
NKNK KE40K-prefix
RINARINA EH40
GB 712GB 712 EH40Chinese national standard

The table maps designations, not certificates. Every grade in it is built on the same IACS unified requirement, so chemistry, tensile and impact values line up closely; what differs is who tests, who stamps and which rule book the yard’s approved plan cites.

A plate can carry ASTM A131 EH40 plus one or more society marks when the mill holds the approvals and each surveyor witnesses the tests before shipment. Ordering the extra marks after rolling is not possible.

Choosing ASTM A131 EH40 within the A131 grade matrix

Read the series as a grid: across (AH40, DH40, EH40, FH40) the test temperature falls; down (EH32, EH36, EH40) the yield rises. A higher letter at the same level is normally accepted as a substitute; a lower letter or lower level is not.

Typical uses of EH40: crack-arrest strakes, Great Lakes and Alaskan service, ice-strengthened hulls and cold-exposed offshore structure.

Why not more strength? A131 stops at level 40. If a design needs 420 N/mm² or above, it leaves A131 and moves to a class-society extra-high-strength grade or another ASTM product specification; there is no “A131 AH420”.

Cutting, forming and welding ASTM A131 EH40

Weld EH40 with low-hydrogen consumables qualified for higher-strength hull steel — typically AWS E7018-1, E71T-1/-9 or F7A/P classes with impact properties at or below −40 °C [−40 °F] in the weld metal (consumable choice per WPS — confirm).

TMCP plate at level 40 has a low carbon equivalent (about Ceq 0.40 % up to 50 mm), so preheat can often be reduced, but high-heat-input processes such as electrogas or one-side SAW need a procedure qualified on plate from the same route. Do not line-heat TMCP plate above the mill’s stated limit (often quoted near 650 °C — UNCERTAIN, mill-specific).

ASTM A131 EH40 mill test report, marking and receiving checks

A6/A6M requires a test report showing the specification and year, grade, heat number, heat analysis, tensile results, impact results, condition of supply and any supplementary requirements. Ask for the report before shipment and check it against the purchase order line by line.

Plates are marked with the manufacturer’s name or brand, heat number, specification and grade — for example “A131 EH40” — and, where class certified, the society stamp. On receipt check the stencil, match heat and plate numbers, confirm −40 °C [−40 °F] and measure thickness at several points.

Electronic MTRs. A6/A6M allows the test report to be transmitted electronically provided it carries the same content and is traceable to the mill’s quality system. Keep the PDF with the heat number in the file name — classification surveyors and US Coast Guard plan reviewers ask for it years later.

ASTM A131 EH40 stock, sizes and lead time

Thickness (mm)Width (mm)Length (mm)ConditionApprox. qty
61829 / 24386096–12192N / TMCP100+ t
824386096–12192N / TMCP120+ t
1024386096–12192N / TMCP150+ t
122438 / 30486096–12192N / TMCP200+ t
162438 / 30486096–12192N / TMCP150+ t
2024386096–12192N / TMCP120+ t
2524386096–12192N / TMCP100+ t
3224386096–12192N / TMCP60+ t
4024386096–12192N / TMCP40+ t
5024386096–12192N / TMCP30+ t

Widths of 1829, 2438 and 3048 mm [72, 96, 120 in.] follow North American plate practice; metric widths are also available. Quantities change weekly — confirm before booking.

Non-stock sizes go into the next mill campaign: about 4–7 weeks plus freight (commercial estimate).

Processing. We cut EH40 to drawing by plasma or oxy-fuel, bevel, shot-blast and prime, and transfer the heat number, grade and specification to every cut piece so the mill test report stays valid for each part.

Mistakes we see on ASTM A131 EH40 purchase orders

  • Ordering ASTM A36 or A572 Gr. 50 when the plan says EH40
  • Writing only “A131 40” so the letter is undefined
  • Accepting a mild-grade report against a higher-strength order
  • No Ceq on the report for TMCP plate
  • Assuming A131 alone satisfies a classed-hull plan
  • Impact band for the delivered thickness not checked

A36 and A572 are building and bridge steels; they share yield levels with some A131 grades but not the hull-steel deoxidation, letter-graded toughness or marking. They are not substitutes on a ship plan.

The one we see most. A purchase order reading only “A131 40” or “A131 high-strength” — without the E letter the impact temperature is undefined and the mill will price, and test, the cheapest letter.

Ordering information for ASTM A131 EH40

A6/A6M lists the information the purchaser must supply; A131 adds grade-specific items. Missing ordering information is the most common reason a mill delivers something technically compliant but commercially wrong.

Sample line: “Plate, ASTM A131/A131M-xx EH40, TMCP, 12.7 × 2438 × 12192 mm [1/2 × 96 × 480 in.], 40 pcs, SI governs, mill test report per A6/A6M, ABS certificate, UT per A578 Level B” — then send it to SHH STEEL.

Purchase-order checklist (A131/A6 ordering information):

  • Specification and year: ASTM A131/A131M-xx (state A131 or A131M units)
  • Grade: EH40
  • Quantity (weight or pieces), dimensions and thickness tolerance basis per A6/A6M
  • Condition of supply / heat treatment (CR, N or TMCP as permitted; state TMCP if Ceq matters)
  • Impact test frequency and orientation where the order requires more than the basic rule
  • Supplementary requirements (e.g. UT, through-thickness, product analysis) by number from A6/A6M
  • Certification: mill test report, ABS (or other society) witness if required, EN 10204 3.1/3.2 if requested
  • Marking, packing and destination

FAQ

What does EH40 mean in ASTM A131?
H marks higher strength, E is the toughness letter (impact at −40 °C [−40 °F]) and 40 is the strength level (390 MPa [57 ksi] yield). The naming matches ABS and IACS, so the grade reads the same on a US mill test report and a class drawing. Level 40 (390 MPa [57 ksi]) is the top of A131. It appears in heavily loaded decks, hatch coamings and offshore structure where level-36 plate would become uneconomically thick. For buyers this means one rule: write the full designation EH40. The letter controls the impact temperature (−40 °C [−40 °F]) and the number controls yield; dropping either leaves the mill free to choose. A131 has no extra-high-strength grades, so the series ends at EH40 and any heavier requirement belongs to a different specification. On drawings and cutting lists, keep the A131 prefix too, so the plate is not confused with a society-only grade.
What strength and toughness does EH40 guarantee?
Yield ≥ 390 MPa, tensile 510–650 MPa [74–94 ksi], elongation ≥ 19 % in 200 mm. Charpy average at −40 °C [−40 °F] rises from 39 J (≤ 50 mm) to 55 J (70–100 mm) longitudinal, one value down to 70 % of the average. The impact energy steps up with thickness because thicker plate has more constraint at the notch. For EH40 used in crack-arrest strakes and winter service, check that the delivered thickness falls in the band the report covers; a 52 mm plate tested as if it were 50 mm is a non-conformance, even if the numbers look good.
Is EH40 the same as ASTM A572 Grade 50 or A36?
No. A572 and A36 are building and bridge steels. EH40 adds fine-grain practice, letter-graded impact testing at −40 °C [−40 °F] and ship-plate marking, and it is what a hull plan requires. A572 Gr. 50 may have a similar yield, but it is not a substitute. The temptation is strongest at level 40, where A572 or similar plate may be cheaper and quicker. It still fails a hull plan: no letter-graded impact test, no fine-grain requirement specific to ship steel and no ship-plate marking. Keep A572 for shore structures, crane foundations and tooling.
Is TMCP EH40 easier to weld?
Usually yes: TMCP plate is made with a lower carbon equivalent — about Ceq 0.40 % up to 50 mm and 0.42 % at 50–100 mm — so preheat can often be reduced. The qualified WPS still governs. EH is where owners, flag administrations and the classification plan most often insist on per-plate testing and full traceability. For EH40 ask for Ceq to two decimals on the report and, if your procedure was qualified on Pcm, for Pcm as well. Thick EH40 welded with high heat input should be covered by a procedure qualified on plate from the same mill and route; a TMCP procedure does not automatically cover normalized plate.
Which grades can replace EH40?
A higher letter at the same level — FH at level 40 — can normally stand in for EH40; a lower letter or level cannot. A131 has no grade above level 40, so heavier-duty needs move to a society extra-high-strength grade. Substitution should be recorded: a mill that ships a higher letter than ordered must still print EH40 (or both grades) on the report and stencil. For classed work the surveyor accepts upward substitution at the same level as a matter of course; downward never.
How do I get EH40 with ABS certification?
Order “ASTM A131 EH40 / ABS EH40” before rolling from an ABS-approved mill. The surveyor witnesses or audits the tests, the plate gets both stencils, and the mill test report and ABS certificate are issued for the same heat. It cannot be added after delivery. For EH40 the surveyor’s involvement adds a few days to testing but nothing to rolling. Mills with ABS approval for the grade and thickness are the realistic choice; ask for the approval scope early, especially for heavy gauges.
What must the mill test report show?
Specification and year, grade EH40, heat and plate numbers, heat analysis including Nb, V, Ti and Al, Ceq for TMCP plate, tensile and −40 °C [−40 °F] impact results, condition of supply and any supplementary requirements (UT, through-thickness) required by the order under A6/A6M. For EH40 we check the report against the order before release: grade and letter, thickness band versus impact results, Ceq for TMCP plate and the supplementary requirements. Missing items are corrected by the mill’s quality system before shipment, not after arrival at the yard.
What are sizes, lead times and payment terms?
Stock covers about 6–50 mm in 1829–3048 mm widths and 6–12 m lengths; rolled sizes take about 4–7 weeks plus freight (estimate). Payment by T/T with balance after inspection, or L/C at sight; third-party inspection on request. For EH40 we cut, bevel, shot-blast and prime in our own workshop and transfer heat numbers to every piece. Mixed sizes can share a container; long or heavy plate ships break bulk. Quantities, weights and the document list are confirmed in writing before loading. Each bundle is tagged with specification, grade, heat and size so the yard can store it straight into the right rack.

Conclusion

ASTM A131 EH40 is the higher-strength grade of ASTM A131/A131M, the US purchase specification for ship structural steel aligned with the ABS Rules: yield 390 MPa [57 ksi], tensile 510–650 MPa, impact −40 °C [−40 °F]. Order it by specification, year and grade, with A6/A6M ordering information complete.

SHH STEEL supplies ASTM A131 EH40 with mill test reports, dual ABS/class certification on request, cutting and UT. Send grade, sizes, quantities and port for a quotation.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *



    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *



      X