LR EH32 Steel Plate | LR/EH32 Marine Steel Plate
What is LR EH32 / LR/EH32 marine steel plate?
LR EH32, often written LR/EH32 on mill certificates and plate markings, is a higher-strength hull structural steel under Lloyd’s Register Rules for the Manufacture, Testing and Certification of Materials, which implement IACS UR W11 for the AH–FH 32/36/40 family. Strength level 32 means minimum yield 315 N/mm², tensile 440–590 N/mm² and elongation 22 % min. (A5). The letter EH fixes Charpy V-notch testing at −40 °C. In commercial enquiries it is called LR EH32 or LR/EH32 marine steel plate.
Equivalent grades: LR EH32 ≈ ASTM A131 Grade EH32 ≈ ABS EH32 ≈ DNV NV E32 ≈ BV EH32 ≈ CCS E32 / EH32 ≈ NK KE32 ≈ KR RE32 ≈ RINA EH32 ≈ GB 712 Grade EH32 (all class-approved, stamped by the issuing society).
LR/EH32 is selected when scantlings need the higher yield of the 32 band and the material class assigns −40 °C toughness. Ordinary-strength LR Grade A–E stay at 235 N/mm² yield and cannot replace EH32 without a drawing change. Within the 32 band, letter choice is toughness: AH 0 °C → DH −20 °C → EH −40 °C → FH −60 °C; within the EH letter, strength steps 32 → 36 → 40 raise yield from 315 to 355 to 390 N/mm².
Plates that pass mill tests under Lloyd’s Register survey are die-stamped or stencilled LR EH32 or LR/EH32 (plus Z or U where through-thickness or ultrasonic requirements apply) and are supplied with a mill certificate the LR Surveyor endorses. SHH STEEL supplies LR/EH32 from Chinese mills that hold Lloyd’s Register works approval for the grade, from stock in common sizes or from a mill rolling cycle, with LR survey arranged at the mill.
LR LR/EH32 plate: specification summary
| Item | LR LR/EH32 / EH32 data |
|---|---|
| Rule basis | Lloyd’s Register Rules for Materials; IACS UR W11 higher-strength Grade EH32 |
| Strength level | higher strength 32, yield 315 N/mm² min., tensile 440–590 N/mm² |
| Toughness class | EH → Charpy at −40 °C |
| Plate thickness primarily covered | up to 100 mm under IACS UR W11 scope for plates; greater thickness by special consideration (see UNCERTAIN) |
| Deoxidation | killed, fine grain practice (UR W11) |
| Impact test | Charpy V at −40 °C; frequency and supply condition per UR W11 tables |
| Marking | LR EH32 / LR/EH32; plus Z / U / TM where ordered and qualified |
| TMCP Ceq (indicative UR W11 / industry practice) | ≤ 0.36 % for t ≤ 50 mm; ≤ 0.38 % for 50 < t ≤ 100 mm (TM steels) — confirm on mill approval / PO |
| Thickness tolerance | IACS UR W13 as adopted by LR (minus tolerance commonly 0.3 mm class — confirm on PO; see UNCERTAIN) |
| Certificate | mill certificate endorsed by the LR Surveyor; EN 10204 3.1 / 3.2 on request |
Size range. Common market thicknesses for EH32 are about 6–80 mm (heavier plates available as per mill approval), widths 1500–3500 mm. Exact maximum thickness for a given delivery condition is as per standard and mill certificate / LR works approval. Ask for confirmation above 100 mm.
LR EH32 / LR/EH32 chemical composition (heat and product analysis)
| Element | Heat (ladle) analysis, % | Product (check) analysis, % | Note |
|---|---|---|---|
| C | 0.18 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | AH/DH/EH group |
| Mn | 0.90–1.60 (AH ≤12.5 mm may be 0.70 min.) | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | AH ≤12.5 mm may use 0.70 % Mn min. |
| Si | 0.10–0.50 | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | min. waived if acid-soluble Al ≥ 0.015 % |
| P | 0.035 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | |
| S | 0.035 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | |
| Al (acid soluble) min. | 0.015 min. acid-soluble (or total Al per UR W11 fine-grain practice) | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | grain refining |
| Nb | 0.02–0.05 when used singly | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | when used singly; combined minima in UR W11 |
| V | 0.05–0.10 when used singly | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | when used singly |
| Ti | 0.02 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | need not be reported unless intentionally added |
| Cu | 0.35 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | |
| Cr | 0.20 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | |
| Ni | 0.40 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | |
| Mo | 0.08 max. | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | |
| N | — | numeric tolerance not tabulated in LR Rules for Materials – agree on order / mill certificate | not specified as a max in AH/DH/EH column |
Product (check) analysis column: LR Rules for Materials specify heat (ladle) limits; no numeric product-analysis tolerance is tabulated in the rule text reviewed, so product (check) limits are agreed on the order or taken from the approved mill specification and certificate.
Source: IACS UR W11 higher-strength chemistry tables (ladle samples) — the chemistry Lloyd’s Register applies to LR/EH32. AH/DH/EH share one chemistry column; FH is tighter on C, P, S and adds N control with higher Ni allowance. Toughness is differentiated by impact temperature and supply routes, not by separate C/Mn caps within AH/DH/EH. Product (check) analysis numeric tolerances are not tabulated in UR W11; when required, agree tolerances at enquiry. TMCP steels must also meet the applicable Ceq / Pcm limits on the mill approval — ask for Ceq on the certificate.
LR LR/EH32 tensile properties
| Property | Requirement (IACS UR W11) |
|---|---|
| Tensile strength Rm | 440–590 N/mm² |
| Yield strength ReH | 315 N/mm² min. |
| Elongation A5 | 22 % min. |
| Impact test temperature | −40 °C |
Alternative flat-specimen elongations by thickness (indicative UR W11 / industry table for strength 32):
| Thickness (mm) | ≤5 | >5–10 | >10–15 | >15–20 | >20–25 | >25–30 | >30–40 | >40–50 |
|---|---|---|---|---|---|---|---|---|
| Elongation min. % | 14 | 16 | 17 | 18 | 19 | 20 | 21 | 22 |
Same tensile band applies to AH/DH/EH/FH 32; only impact temperature and chemistry group (FH vs AH/DH/EH) change across the letter.
LR LR/EH32: Charpy at −40 °C and supply condition
| Thickness | Long. avg. at −40 °C | Trans. avg. at −40 °C |
|---|---|---|
| t ≤ 50 mm | 31 J | 22 J |
| 50 < t ≤ 70 mm | 38 J | 26 J |
| 70 < t ≤ 100 mm | 46 J | 31 J |
Source: IACS UR W11 impact table for higher-strength Grade EH32 (full-size; either direction acceptable unless specified). Energies rise with thickness — a 60 mm plate must meet higher values than a 20 mm plate at the same −40 °C. Condition of supply and impact lot size depend on grain-refining practice and thickness (AR/CR/N/TM/QT as permitted). For TMCP EH32, respect Ceq caps ≈ 0.36 % (t≤50) / 0.38 % (50
Thickness tolerance and surface condition
Lloyd’s Register applies IACS UR W13 thickness tolerances unless the PO states otherwise (often 0.3 mm minus class — confirm on PO; see UNCERTAIN). Plus/flatness/width/length per agreed standard (ASTM A6 or EN 10029). Surface quality per EN 10163 or equivalent accepted by LR; state primer/surface class on receipt if needed.
LR LR/EH32 plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Condition | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1800 / 2000 | 6000 / 8000 | AR / CR / N / TM | 100+ t | China |
| 8 | 1800 / 2000 | 8000 / 12000 | AR / CR / N / TM | 200+ t | China |
| 10 | 2000 / 2200 | 8000 / 12000 | AR / CR / N / TM | 200+ t | China |
| 12 | 2000 / 2200 / 2500 | 12000 | AR / CR / N / TM | 200+ t | China |
| 14 | 2000 / 2200 | 12000 | AR / CR / N / TM | 100+ t | China |
| 16 | 2000 / 2500 | 12000 | AR / CR / N / TM | 200+ t | China |
| 20 | 2000 / 2500 | 12000 | AR / CR / N / TM | 100+ t | China |
| 25 | 2200 / 2500 | 12000 | AR / CR / N / TM | 100+ t | China |
| 30 | 2200 | 10000 / 12000 | AR / CR / N / TM | 100+ t | China |
| 40 | 2200 | 10000 | AR / CR / N / TM | 50+ t | China |
| 50 | 2200 | 8000 / 10000 | AR / CR / N / TM | 50+ t | China |
Quantities are approximate and change daily (indicative — confirm before booking); all stock plates carry LR/EH32 marking and LR-endorsed mill certificates when sold as LR class plate. Sizes outside the table (for example 3000 mm width, 60–100 mm thickness, or fixed lengths for a cutting plan) are produced in the next mill rolling cycle, typically 3–6 weeks including LR survey. Send your size list and we will reply with what is in stock and what must be rolled.
Packing. Plates are bundled by size with steel strapping, marked with heat number, grade and LR stamp, and shipped in containers (up to about 11.8 m) or break bulk for longer plates.
LR LR/EH32 equivalents in other rules and standards
| Standard / society | Designation | Comment |
|---|---|---|
| LR (Lloyd’s Register) | LR/EH32 (LR EH32) | this page; stamped under LR survey |
| ASTM A131/A131M | ASTM A131/A131M Grade EH32 | A131 lists AH–FH 32/36/40; product standard only |
| ABS | ABS EH32 | IACS UR W11 higher-strength; live product page |
| DNV | DNV NV E32 | IACS UR W11; live product page |
| BV | BV Grade EH32 | IACS UR W11; category link only |
| CCS | CCS EH32 | IACS UR W11; category link only |
| NK (ClassNK) | NK KE32 | ClassNK KE32 |
| KR | KR RE32 | KR RE32 |
| RINA | RINA Grade EH32 | confirm exact designation per RINA rules |
| GB 712 | GB 712 Grade EH32 | not class approval by itself |
| Structural (indicative) | S275JR | land structural; no class marking |
These are comparisons, not substitutions. Multi-class stamps require joint survey before rolling.
LR LR/EH32 vs other LR hull grades
Pick EH32 when the drawing specifies higher-strength grade EH32 (or the society equivalent). Do not substitute ordinary Grade A/B unless the designer recalculates scantlings — yield differs (315 vs 235). Within the 32 band, letter choice is toughness: AH 0 °C → DH −20 °C → EH −40 °C → FH −60 °C. Within the EH letter, strength steps 32 → 36 → 40 raise yield from 315 to 355 to 390 N/mm².
For yields above 390 N/mm² Lloyd’s Register / IACS move to extra-high strength (UR W16 naming — LR uses AH42…AH69, not AH420 / AH70).
When LR LR/EH32 is the right choice: typical uses are special and primary category members, crack-arrest strakes, and hull structure for cold-route or ice-strengthened vessels needing −40 °C toughness. The Charpy temperature (−40 °C) is fixed by the letter, and the strength by the number (ReH 315 N/mm²). Pick the strength from the scantling calculation and the letter from the material class and design temperature on the approved drawing.
Applications, cutting and welding of LR LR/EH32
Typical uses: special and primary category members, crack-arrest strakes, and hull structure for cold-route or ice-strengthened vessels needing −40 °C toughness; weight-saving vs ordinary-strength plate in large tankers, bulkers and container ships. See offshore platform steel plates when primary offshore grades apply.
Welding: higher-strength hull steels need approved higher-strength consumables matched to −40 °C weld-metal toughness; preheat and heat input follow the approved WPS and often track Ceq/Pcm from the mill certificate. TMCP EH32 must respect the Ceq caps noted above. Cutting by oxy-fuel/plasma/laser is routine; thick FH plate may need hydrogen control — follow mill recommendations.
Processing notes for LR/EH32: cold forming is routine within normal shipyard radii. Line heating and fairing of TMCP plate should stay within the temperature limits recommended by the mill, because overheating can reduce the strength gained in controlled rolling. Check the delivery condition on the certificate before planning hot forming.
Certificates, LR survey and third-party inspection
Every plate is tested and marked at the mill under Lloyd’s Register survey; the mill certificate lists heat number, ladle chemistry, Ceq where applicable, tensile results (ReH ≥ 315 N/mm², Rm 440–590 N/mm², A ≥ 22 %), Charpy at −40 °C, delivery condition and plate numbers, endorsed by the Surveyor. Optional EN 10204 3.2, UT (U), Z-direction, multi-class.
On receipt: verify LR/EH32 stamp, −40 °C impact data, energies for the delivered thickness band, thickness within UR W13 / PO tolerance, LR endorsement present.
Charpy acceptance for LR/EH32 by thickness (IACS UR W11; actual results as per standard and mill certificate):
| Thickness t (mm) | Test temperature | Average energy, longitudinal (J min.) | Average energy, transverse (J min.) |
|---|---|---|---|
| t ≤ 50 | −40 °C | 31 | 22 |
| 50 < t ≤ 70 | −40 °C | 38 | 26 |
| 70 < t ≤ 100 | −40 °C | 46 | 31 |
If UT or 3.2 was ordered, check the UT report and inspector’s plate list as well.
Common mistakes when ordering LR EH32 / LR/EH32
- Ordering “LR 32” without the letter (EH/…) — toughness class missing
- Accepting ordinary-strength Grade A/B certificates for a EH32 PO
- Ignoring TMCP Ceq caps on TM plate
- Substituting a different letter (e.g. AH for EH) without drawing approval
- Coil-cut plate without coil approval
- Missing LR endorsement on the MTC
Write grade, delivery condition, impact temperature and certificate type into the PO.
Sourcing LR LR/EH32: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Fake class plate | LR-approved mills only; traceable LR/EH32 stamp + certificate; 3.2 on request |
| Payment risk | T/T or L/C; inspection before balance |
| Mixed sizes / grades | EH32 combined with LR Grade A/B/D/E or other AH–FH sizes in one container |
| Lead time visibility | weekly photo updates from dedicated coordinator |
| Prep before ship | cutting, bevelling, drilling, machining in our workshop |
How to order LR LR/EH32 plate
Specify LR EH32 (LR/EH32), delivery condition (AR/CR/N/TM/QT as applicable), thickness × width × length × qty, Z/U, multi-class, certificate type, port. Send to SHH STEEL.
Sample PO line: “Steel plate to Lloyd’s Register Rules for Materials, Grade EH32 (LR/EH32), delivery condition [AR/CR/N/TM/QT], 20 × 2500 × 12000 mm, 30 pcs, marked LR EH32 / LR/EH32, certificate endorsed by LR Surveyor, EN 10204 3.2 [if required], UT [if required], CIF [port].”
FAQ
Conclusion
LR EH32 / LR/EH32 is higher-strength hull steel under Lloyd’s Register Materials rules and IACS UR W11: yield 315 N/mm², tensile 440–590 N/mm², Charpy at −40 °C, marking LR/EH32. Lock on the order: delivery condition, impact lot size, TMCP Ceq if TM, product analysis if needed, multi-class and 3.2.
SHH STEEL supplies LR/EH32 plate rolled by Chinese mills that hold Lloyd’s Register works approval for the grade, so every plate carries the LR/EH32 stamp and a Surveyor-endorsed certificate traceable to its heat. Common thicknesses are available from stock; other sizes are scheduled into the mill rolling cycle with LR survey arranged at the mill. On request we add EN 10204 3.2 certificates with third-party witness (TÜV, SGS, BV or another agency) and joint certification with ABS, DNV, BV, CCS, NK, KR or RINA.
We accept T/T or L/C payment, with inspection before the balance is paid. Small quantities in several sizes, or LR/EH32 mixed with LR Grade A/B/D/E or other AH–FH sizes, can be combined in one container. A dedicated coordinator sends production and shipping updates with photos, and our own workshop cuts to size, bevels, drills and machines plates before shipment so they arrive ready for fabrication.
Request a quotation: send SHH STEEL the grade (LR/EH32 / LR EH32), thickness, width, length, quantity per size and destination port, plus any multi-class, Z/U or 3.2 certificate requirement. We reply with price, available stock and lead time.