JIS G3602 NW6022 (C22) Nickel Alloy Clad Steel Plate
What is JIS G3602 NW6022 (alloy C-22) nickel alloy clad steel plate?
JIS G3602 NW6022 (alloy C-22) nickel alloy clad steel plate is a composite plate in which NW6022 (alloy C-22, UNS N06022) to JIS H4551 is metallurgically bonded to a JIS carbon or low-alloy steel base, ordered to JIS G3602 “Nickel and nickel alloy clad steels”. The base, usually a pressure vessel steel such as SGV480, carries the load; the NW6022 face resists the process medium. The standard covers clad steel for pressure vessels, nuclear reactors and storage tanks.
NW6022 is the JIS designation of alloy C-22, the nickel-chromium-molybdenum-tungsten alloy often sold as Hastelloy C-22. With more chromium than C-276 it handles oxidizing and mixed media better while keeping good resistance in reducing acids, and it is specified on Japanese-standard projects for pharmaceutical, flue gas and mixed-acid equipment.
A typical order reads: JIS G3602 B1, NW6022 3 mm + SGV480 20 mm, 2000 × 6000 mm. That line fixes the method and class, both grades, both thicknesses and the plate size, and it is the format we ask for when quoting.
SHH STEEL can produce JIS G3602 NW6022 clad plate in China, mainly by explosion bonding and explosion-rolling, on the JIS base steel your order names. We work to JIS G3602:2012, confirmed in 2017, and certify each plate to its tests.
JIS G3602 types, classes and symbols
JIS G3602 uses the same classification as the other Japanese clad steel standards: a letter code for the manufacturing method and a number for the class. The method codes below are taken from the standard’s Table 1.
| Manufacturing method | Class 1 | Class 2 |
|---|---|---|
| Rolled clad steel | R1 | R2 |
| Explosion-rolled clad steel | BR1 | BR2 |
| Diffusion-rolled clad steel | DR1 | DR2 |
| Overlay-rolled clad steel | WR1 | WR2 |
| Cast-in rolled clad steel | ER1 | ER2 |
| Explosion clad steel | B1 | B2 |
| Diffusion clad steel | D1 | D2 |
| Weld overlay clad steel | W1 | W2 |
| Class | Meaning in JIS G3602 |
|---|---|
| Class 1 (…1) | Designed with the cladding included as a strength member, and clad steel for special uses, such as high-temperature service or severe working during fabrication |
| Class 2 (…2) | All other clad steel, for example where the cladding is a corrosion allowance or replaces a lining |
The class decides how the plate is tested. Under the Table 2 notes, class 2 clad steel, clad steel on a forged or cast base, and any plate where the purchaser asks for it are tensile tested on the base alone, against the base standard; a full-thickness test can replace that by agreement. Class 1 is tested as a composite against a thickness-weighted strength. The shear test, at least 200 N/mm², applies to rolled, explosion and diffusion clad steel; weld overlay clad steel has no shear requirement.
For NW6022 clad plate, explosion clad (B1 or B2) is the usual route for tube sheets and heavy plate, and explosion-rolled (BR1 or BR2) for larger, thinner plates. Class 2 suits vessels that treat the C-22 as a corrosion barrier; class 1 is for hot service, heavy forming or designs that count the cladding.
NW6022 cladding and JIS base steels
JIS G3602 takes the chemistry and properties of each layer from its own product standard (clause 10, materials). Nickel and nickel alloy claddings come from two Japanese standards: JIS H4551 for nickel and nickel alloy plate (the NW designations) and JIS G4902 for corrosion- and heat-resisting superalloy plate (the NCF designations). NW6022 is a JIS H4551 grade.
| Base steel standard (cited in JIS G3602) | Typical grades | Use |
|---|---|---|
| JIS G3118, carbon steel plates for pressure vessels for intermediate and moderate temperature | SGV480, SGV410, SGV450 | Most clad pressure vessels |
| JIS G3103, carbon and molybdenum steel plates for boilers and pressure vessels | SB410, SB450, SB480 | Boilers, vessels |
| JIS G3115, steel plates for pressure vessels | SPV355, SPV235, SPV315 | Higher-yield vessel shells |
| JIS G3126, carbon steel plates for low temperature pressure vessels | SLA grades | Low-temperature service |
| JIS G4109, Cr-Mo steel plates for boilers and pressure vessels | SCMV grades | Elevated-temperature service |
| JIS G3106, rolled steels for welded structure | SM400, SM490 | Non-pressure tanks and structures |
Why NW6022 (Hastelloy C22) is used
Alloy C-22 contains 20.0 to 22.5 % chromium, 12.5 to 14.5 % molybdenum, 2.5 to 3.5 % tungsten and 2.0 to 6.0 % iron, with nickel as the balance. Carbon is limited to 0.015 % and silicon to 0.08 %.
The higher chromium improves resistance to oxidizing acids and oxidizing salts in chloride solutions, while molybdenum and tungsten keep resistance to reducing acids and to pitting and crevice corrosion. C-22 is also thermally stable, so the heat-affected zones of welds keep their resistance.
Where N06022 cladding performs and where it does not
| Medium or condition | N06022 cladding |
|---|---|
| Oxidizing acids with chlorides | Very good |
| Wet chlorine with oxidizing ions | Very good |
| Reducing acids | Good |
| Pitting and crevice corrosion in chlorides | Excellent |
| FGD acid condensate | Excellent |
| Strong hot hydrochloric acid | Good; Ni-Mo alloys may be better |
Choosing the base
SGV480 and SB410 are the usual bases for JIS clad vessels, with SPV355 where higher yield reduces thickness and SCMV grades where the design temperature needs Cr-Mo steel. When an export project asks for “JIS G3602 NW6022” without naming a base, we confirm the base grade and its standard before quoting, because the base decides the strength, the heat treatment and the welding procedure.
Most vessel shells use 2 to 3 mm of N06022; tube sheets often need more so that tube-to-tubesheet welds sit entirely in the alloy. Thicker cladding is made by explosion welding.
Chemical composition of NW6022 cladding and the base
Under JIS G3602 each layer meets the chemistry of its own standard; for weld overlay types the overlay chemistry is agreed between the parties. The cladding table gives the ASTM limits of UNS N06022 for reference, because most export orders are checked against them; a JIS H4551 NW6022 certificate reports the limits of the JIS standard, and a dual-certified heat must meet both.
Hastelloy C22 (N06022) cladding, ASTM limits for reference
| Element | N06022, % |
|---|---|
| Nickel (Ni) | Balance |
| Chromium (Cr) | 20.0 – 22.5 |
| Molybdenum (Mo) | 12.5 – 14.5 |
| Tungsten (W) | 2.5 – 3.5 |
| Iron (Fe) | 2.0 – 6.0 |
| Cobalt (Co) | 2.5 max |
| Manganese (Mn) | 0.50 max |
| Vanadium (V) | 0.35 max |
| Carbon (C) | 0.015 max |
| Silicon (Si) | 0.08 max |
| Phosphorus (P) | 0.02 max |
| Sulfur (S) | 0.02 max |
The limits are those of ASTM B575 for UNS N06022, given for reference. A JIS H4551 certificate reports the JIS limits for NW6022.
Example base: SGV480 (JIS G3118)
| Element | SGV480 heat analysis, % (JIS G3118) |
|---|---|
| C, 6 – 12.5 mm | ≤ 0.27 |
| C, over 12.5 – 50 mm | ≤ 0.28 |
| C, over 50 – 100 mm | ≤ 0.30 |
| C, over 100 – 200 mm | ≤ 0.31 |
| Si | 0.15 – 0.40 |
| Mn | 0.85 – 1.20 |
| P, S | Per the JIS G3118 edition ordered |
For other bases, such as SB410 or SPV355, the chemistry is that of JIS G3103 or JIS G3115 and is reported on the base mill certificate. Keep the base sulfur low where the plate will be heavily formed, because it helps both bonding and later welding.
Mechanical properties, bend and shear tests
JIS G3602 Table 2 sets the requirements for the clad steel as a product.
| Property | Rolled, explosion and diffusion clad steel | Weld overlay clad steel |
|---|---|---|
| Tensile strength | Not less than σB = (t1·σB1 + t2·σB2) / (t1 + t2) | Same |
| Elongation | Not less than the lower of the base and cladding specified values | Same |
| Bend, 180° | Face bend: inside radius per the cladding standard; back bend: per the base standard; never less than 1 × total thickness; no cracks | Face bend, inside radius 2 × total thickness; cracks under 3 mm |
| Shear strength | ≥ 200 N/mm² | Not specified |
In the formula, σB1 is the specified minimum tensile strength of the base, σB2 that of the cladding, and t1 and t2 the base and cladding thicknesses. For class 2 clad steel, for forged or cast bases, or when the purchaser specifies it, the tensile test is made on the base only, and the yield and tensile strength must meet the base standard.
A face bend may be left out when the cladding standard has no bend requirement, and a back bend when the base standard has none. A side bend can replace the face bend; then no crack of 1.6 mm or more is allowed on the outside of the bend.
N06022 cladding strength (ASTM B575, for reference)
| Property | Hastelloy C22 (N06022) |
|---|---|
| Tensile strength | 690 MPa min |
| Yield strength (0.2 %) | 310 MPa min |
| Elongation | 45 % min |
| Hardness | Not specified for acceptance |
Example base: SGV480
| SGV480 property (JIS G3118) | Requirement |
|---|---|
| Yield point or proof stress | ≥ 265 N/mm² |
| Tensile strength | 480 – 590 N/mm² |
| Elongation, 6 – 40 mm, No. 1A test piece | ≥ 17 % |
| Elongation, over 50 mm, No. 10 test piece | ≥ 21 % |
| Delivery | As rolled up to 38 mm; normalized over 38 mm |
Worked example for class 1, 3 mm NW6022 on 20 mm SGV480, using the reference cladding values above (ASTM B575 values): σB = (20 × 480 + 3 × 690) / 23 = 507 N/mm². The certificate uses the JIS H4551 minimum for NW6022, so confirm the figure against the edition ordered. Elongation must meet the lower of the two specified values. If the design also needs a composite yield value, the same weighting gives about (20 × 265 + 3 × 310) / 23 = 271 N/mm², a planning estimate only. For class 2, the SGV480 alone is tested against 265 N/mm² and 480 to 590 N/mm².
Bonding, ultrasonic inspection and corrosion testing
JIS G3602 clause 7 sets the bonding condition, and clause 12 lists the tests, with the methods taken from JIS G0601, the Japanese standard for testing clad steel. Bond quality is checked by ultrasonic testing over the plate and graded by the extent of unbonded area; the grade and scanning coverage should be stated in the order, especially for tube sheets that will be drilled.
Corrosion tests of the NW6022 layer are not a routine product test, so if the service needs one, name the method, the acceptance and the condition of the samples: as bonded, or after the heat treatment the vessel will receive. For nickel claddings the most common request is a test after simulated PWHT.
C-22 is a low-carbon alloy with good thermal stability, which helps it keep its corrosion resistance after the heat of bonding. Keep later heat treatment short and qualified on coupons, and we report the measured shear values on the certificate.
Clad plate or weld overlay?
C-22 overlay with ERNiCrMo-10 suffers iron dilution like other nickel overlays, and several layers are needed to reach low iron at the surface. An explosion clad N06022 plate puts full-chemistry alloy over the whole wall.
Manufacturing method, heat treatment and delivery
JIS G3602 clause 11 covers the manufacturing method. In practice the delivery condition follows the base steel standard, since the base carries the load: SGV480, for example, is as rolled up to 38 mm and normalized above that. The cladding face is delivered as bonded and cleaned, or as agreed.
JIS G3602 NW6022 clad plate is usually delivered as clad and flattened, or stress relieved by agreement, with the alloy sheet solution annealed before bonding. Long holds at intermediate temperatures can precipitate secondary phases, so qualify any PWHT on coupons and consider a corrosion test of the cladding afterwards.
Keep the nickel face clean before heating
Nickel and its alloys are embrittled by sulfur, phosphorus, lead and other low-melting contaminants picked up at high temperature. Before normalizing, stress relief, hot forming or welding, remove marking crayon, paint, oil and shop dirt from the NW6022 surface, and keep high-sulfur furnace atmospheres away from it. Use sulfur-free markers only.
Dimensions, tolerances and weight
Clause 8 of JIS G3602 sets tolerances for width and length (8.1), thickness (8.2) and flatness (8.3), building on JIS G3193 for hot-rolled plate. The cladding and total thickness tolerances are the ones to confirm at the order stage, because they decide the corrosion allowance actually delivered.
| Item | What to state in the order |
|---|---|
| Cladding thickness | Nominal, and a minimum if the corrosion allowance must be guaranteed |
| Base thickness | Nominal, per the base steel standard |
| Width and length | Finished size, or size before cutting into discs or head blanks |
| Flatness | Standard, or special flatness for tube sheets |
| Surface | Cladding pickled, ground or polished; base as rolled or blasted |
Theoretical weight uses a nominal 8.69 g/cm³ for NW6022 and 7.85 g/cm³ for the carbon steel base. A 3 + 20 mm plate therefore weighs about 3 × 8.69 + 20 × 7.85 = 183.1 kg per square metre, and a 2000 × 6000 mm plate about 2.2 t.
Stock sizes and thickness combinations of JIS G3602 NW6022 clad plate
JIS G3602 NW6022 clad plate is specified by cladding and base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.
| Cladding + base, mm | Total, mm | Typical use |
|---|---|---|
| 2 + 12 | 14 | Scrubbers and ducts |
| 2 + 16 | 18 | Column shells |
| 3 + 20 | 23 | Reactors |
| 3 + 26 | 29 | Larger reactors |
| 4 + 36 | 40 | Heads |
| 5 + 50 | 55 | Thick shells |
| 6 + 60 | 66 | Tube sheets |
| Dimension | Production range |
|---|---|
| Cladding thickness | 2 mm to 20 mm (thicker by explosion bonding on request) |
| Base steel thickness | 6 mm to 200 mm |
| Total thickness | 8 mm to 220 mm |
| Width | 1000 mm to 3000 mm; wider by explosion bonding with welded cladding |
| Length | 2000 mm to 12000 mm |
| Discs and blanks | Round tube sheet blanks and head blanks cut to drawing |
| Location | China |
Welding JIS G3602 NW6022 clad plate
JIS clad steel is welded in the usual clad sequence: weld the carbon steel base first with matching filler, then restore the NW6022 face with nickel alloy filler. Carbon steel filler must not be deposited on the cladding.
- Bevel from the base side and set back the cladding at the root as the procedure requires.
- Weld the base with low-hydrogen carbon steel filler matched to the base grade.
- Back-gouge from the clad side to sound weld metal.
- Restore the cladding with ERNiCrMo-10 (AWS A5.14) or ENiCrMo-10 (AWS A5.11), matching alloy C-22, using at least two layers.
- Check the finished clad-side weld visually and by penetrant testing.
ERNiCrMo-10 matches C-22 and is also used as an over-alloyed filler on C-276. Use low heat input and stringer beads; avoid high interpass temperatures that promote precipitation in the HAZ.
Repair welding of the clad steel itself is covered by JIS G3602 clause 14; repaired areas are checked again before release, and the repair is recorded in the report.
Applications of JIS G3602 NW6022 nickel alloy clad steel plate
JIS G3602 NW6022 clad steel plate is used where the medium swings between oxidizing and reducing conditions, or carries oxidizing contaminants that limit C-276.
- Pharmaceutical and agrochemical reactors.
- Chlorination equipment with oxidizing ions.
- Mixed acid and pickling vessels.
- FGD absorber zones and scrubbers.
- Waste treatment and incineration scrubbers.
- Multipurpose chemical vessels.
Ordering tips
State the full medium analysis, including oxidizing species, the design temperature and whether PWHT is required. For multipurpose vessels list all the products the vessel will see, so the cladding choice covers the worst case.
Tests, inspection, retests and report
JIS G3602 clause 12 lists the tests, clause 13 the inspection, clause 15 retests, clauses 16 and 17 the product symbol and marking, and clause 18 the report.
| Test | Requirement for JIS G3602 NW6022 |
|---|---|
| Chemical analysis | Cladding and base per their own standards |
| Tensile | Composite (class 1) or base only (class 2), per Table 2 |
| Bend | Face and back bends, 180°, per Table 2 |
| Shear | ≥ 200 N/mm² for rolled, explosion and diffusion clad steel |
| Ultrasonic test | Bond inspection per JIS G0601, grade as ordered |
| Dimensions and appearance | Clause 8 tolerances; visual check of both surfaces (clause 9) |
| Corrosion test | NW6022 layer, only when ordered; method and acceptance by agreement |
The inspection document is issued to JIS G0415 / EN 10204 3.1, or 3.2 with third-party inspection. It reports the clad steel symbol, the NW6022 and base grades and heats, thicknesses and all test results.
Equivalent standards and grades
JIS G3602 sits beside the ASTM and Chinese nickel clad plate standards; the test levels differ, so compare before substituting.
| Standard | Bond shear requirement | Classification |
|---|---|---|
| JIS G3602 | ≥ 200 N/mm² (not for weld overlay) | Method code + class 1 / 2 |
| ASTM A265 / ASME SA-265 | ≥ 140 MPa, when specified | UT class as ordered |
| NB/T 47002.2-2019 | 210 MPa benchmark (GB/T 150.2) | Method code + class |
| Layer | JIS | UNS | EN | GB |
|---|---|---|---|---|
| Cladding | NW6022 (JIS H4551) | N06022 | 2.4602 (NiCr21Mo14W) | NS3308 |
| Base | SGV480 (JIS G3118) | SA516 Gr.70 (approx.) | P355GH (approx.) | Q345R (approx.) |
For ASME work the nearest product is SA516 Gr.70 + alloy C-22 to ASME SA-265. Equivalence is approximate. Check chemistry, strength and test requirements against the design code before substituting.
Why order JIS G3602 NW6022 clad plate from SHH STEEL
SHH STEEL is a clad plate manufacturer in China and supplies nickel alloy clad steel to Japanese-standard projects in Asia and beyond. For NW6022 clad plate we can supply alloy C-22 certified to JIS H4551 and, when the heat meets both, to ASTM B575 as well.
- We confirm the method code and class (for example B1 or BR2) and the base grade before production.
- Cladding to JIS H4551 and base to its JIS standard come with traceable mill certificates.
- Each plate is ultrasonically tested, and shear and bend results are reported on the certificate.
- Plates can be cut into tube sheet discs and head blanks.
FAQ
-
Which standard covers the NW6022 cladding?
- NW6022 is a JIS H4551 grade. JIS G3602 takes the cladding chemistry and properties from that standard and adds the clad steel tests: shear, bend, composite tensile and ultrasonic bond inspection.
-
What tensile strength does 3 + 20 mm NW6022 on SGV480 need?
- For class 1, JIS G3602 uses the thickness-weighted average. With SGV480 at 480 N/mm² and the reference NW6022 value of 690 N/mm², that is about 507 N/mm²; confirm with the JIS H4551 minimum. Class 2 is tested on the SGV480 alone.
-
Is JIS G3602 NW6022 the same as ASTM A265 alloy C-22 clad plate?
- They are close equivalents, not identical. JIS G3602 requires at least 200 N/mm² shear for rolled, explosion and diffusion types; ASTM A265 requires 140 MPa only when the shear test is specified. The cladding is certified to JIS H4551 rather than ASTM B575, so cite both only with a dual-certified heat.
-
What is the difference between class 1 and class 2 in JIS G3602?
- Class 1 is clad steel designed with the cladding as a strength member, or for special uses such as high temperature or severe forming. Class 2 covers the rest, typically where the cladding is a corrosion allowance. Class 2 is tensile tested on the base only.
-
What shear strength does JIS G3602 require?
- At least 200 N/mm² for rolled, explosion and diffusion clad steel. Weld overlay clad steel has no shear requirement.
-
What is the HS code for nickel alloy clad steel plate?
- Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The code depends on the base steel and width, so confirm with your customs broker.
-
What should I send for a quotation?
- JIS G3602, the type and class (for example B1), NW6022 cladding thickness, base grade and thickness, width, length, quantity, tests beyond the standard and certificate type.
Request a quotation for JIS G3602 NW6022 (C22) Nickel Alloy Clad Steel Plate
JIS G3602 NW6022 nickel alloy clad steel plate bonds alloy C-22 to a JIS base steel such as SGV480 or SB410. The standard classifies it by method code and class 1 or 2, requires at least 200 N/mm² bond shear for rolled, explosion and diffusion types, and sets thickness-weighted tensile, bend and ultrasonic tests.
Send the type and class, thickness pair, base grade, size and quantity to SHH STEEL, or compare other grades under JIS G3602 and on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.
Contact: admin@steelspecs.com