JIS G3602 NCF625 (Alloy 625) Nickel Alloy Clad Steel Plate

JIS G3602 NCF625 nickel alloy clad steel plate bonds alloy 625 (UNS N06625) to a JIS pressure vessel steel such as SGV480 or SB410. JIS G3602 classifies it by method code and class 1 or 2 and requires at least 200 N/mm² bond shear for explosion and rolled types. SHH STEEL produces it in China on the base your order names.
Keywords
JIS G3602 NCF625 clad plate, alloy 625 clad steel plate, NCF625 + SGV480, JIS G3602 nickel clad steel, nickel alloy clad steel plate
Equivalent Grades:
ASTM A265 / ASME SA-265, NB/T 47002.2; NCF625 = alloy 625 / UNS N06625 / 2.4856 (NiCr22Mo9Nb) / NS3306
Share:
General Description
Material Specification
Base and Cladding Materials
Chemical Composition
Mechanical Properties
Bonding Condition
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is JIS G3602 NCF625 (alloy 625) nickel alloy clad steel plate?

JIS G3602 NCF625 (alloy 625) nickel alloy clad steel plate is a composite plate in which NCF625 (alloy 625, UNS N06625) to JIS G4902 is metallurgically bonded to a JIS carbon or low-alloy steel base, ordered to JIS G3602 “Nickel and nickel alloy clad steels”. The base, usually a pressure vessel steel such as SGV480, carries the load; the NCF625 face resists the process medium. The standard covers clad steel for pressure vessels, nuclear reactors and storage tanks.

NCF625 is the JIS G4902 designation of alloy 625, the nickel-chromium-molybdenum-niobium alloy often sold as Inconel 625. It is the strongest of the common nickel claddings and has the highest pitting resistance of them, so Japanese-standard projects specify it for sea water, acid chloride condensate and flue gas cleaning equipment where stainless and even super duplex claddings are marginal.

A typical order reads: JIS G3602 B1, NCF625 3 mm + SGV480 20 mm, 2000 × 6000 mm. That line fixes the method and class, both grades, both thicknesses and the plate size, and it is the format we ask for when quoting.

SHH STEEL can produce JIS G3602 NCF625 clad plate in China, mainly by explosion bonding and explosion-rolling, on the JIS base steel your order names. We work to JIS G3602:2012, confirmed in 2017, and certify each plate to its tests.

JIS G3602 types, classes and symbols

JIS G3602 uses the same classification as the other Japanese clad steel standards: a letter code for the manufacturing method and a number for the class. The method codes below are taken from the standard’s Table 1.

Manufacturing method Class 1 Class 2
Rolled clad steel R1 R2
Explosion-rolled clad steel BR1 BR2
Diffusion-rolled clad steel DR1 DR2
Overlay-rolled clad steel WR1 WR2
Cast-in rolled clad steel ER1 ER2
Explosion clad steel B1 B2
Diffusion clad steel D1 D2
Weld overlay clad steel W1 W2
Class Meaning in JIS G3602
Class 1 (…1) Designed with the cladding included as a strength member, and clad steel for special uses, such as high-temperature service or severe working during fabrication
Class 2 (…2) All other clad steel, for example where the cladding is a corrosion allowance or replaces a lining

The class decides how the plate is tested. Under the Table 2 notes, class 2 clad steel, clad steel on a forged or cast base, and any plate where the purchaser asks for it are tensile tested on the base alone, against the base standard; a full-thickness test can replace that by agreement. Class 1 is tested as a composite against a thickness-weighted strength. The shear test, at least 200 N/mm², applies to rolled, explosion and diffusion clad steel; weld overlay clad steel has no shear requirement.

For NCF625 clad plate, explosion clad (B1 or B2) is the usual route for tube sheets and heavy plate, and explosion-rolled (BR1 or BR2) for larger, thinner shell plates. Choose class 1 only if the design counts the high-strength 625 layer or the plate will work hot or be heavily formed; otherwise class 2 is normal and keeps the tensile test simple.

NCF625 cladding and JIS base steels

JIS G3602 takes the chemistry and properties of each layer from its own product standard (clause 10, materials). Nickel and nickel alloy claddings come from two Japanese standards: JIS H4551 for nickel and nickel alloy plate (the NW designations) and JIS G4902 for corrosion- and heat-resisting superalloy plate (the NCF designations). NCF625 is a JIS G4902 grade.

Base steel standard (cited in JIS G3602) Typical grades Use
JIS G3118, carbon steel plates for pressure vessels for intermediate and moderate temperature SGV480, SGV410, SGV450 Most clad pressure vessels
JIS G3103, carbon and molybdenum steel plates for boilers and pressure vessels SB410, SB450, SB480 Boilers, vessels
JIS G3115, steel plates for pressure vessels SPV355, SPV235, SPV315 Higher-yield vessel shells
JIS G3126, carbon steel plates for low temperature pressure vessels SLA grades Low-temperature service
JIS G4109, Cr-Mo steel plates for boilers and pressure vessels SCMV grades Elevated-temperature service
JIS G3106, rolled steels for welded structure SM400, SM490 Non-pressure tanks and structures

Why NCF625 (Inconel 625) is used

Alloy 625 contains 20.0 to 23.0 % chromium, 8.0 to 10.0 % molybdenum, 3.15 to 4.15 % niobium plus tantalum and at least 58 % nickel, with iron limited to 5.0 %. The combination of chromium and molybdenum gives resistance to both oxidizing and reducing media and an extremely high resistance to chloride pitting; the high nickel makes it practically immune to chloride stress corrosion cracking.

625 is also strong. Its minimum yield in annealed plate, 379 MPa, is well above that of the stainless steels, which helps the clad face resist erosion in slurries and high-velocity flow. Its weakness, if any, is price; where the medium allows, alloy 825 or a super-austenitic stainless steel costs less.

Where N06625 cladding performs and where it does not

Medium or condition N06625 cladding
Hot sea water and brines Excellent; very high pitting resistance
Acid chloride condensates (FGD) Very good
Phosphoric and dilute sulfuric acid Good
Nitric and oxidizing media Good
Hot concentrated hydrochloric acid Limited; consider nickel-molybdenum alloys
Chloride stress corrosion cracking Practically immune

Choosing the base

SGV480 and SB410 are the usual bases for JIS clad vessels, with SPV355 where higher yield reduces thickness and SCMV grades where the design temperature needs Cr-Mo steel. When an export project asks for “JIS G3602 NCF625” without naming a base, we confirm the base grade and its standard before quoting, because the base decides the strength, the heat treatment and the welding procedure.

Nickel alloy cladding is expensive, so thickness is chosen carefully. Most vessel shells use 2 to 3 mm of N06625; tube sheets often need more so that tube-to-tubesheet welds sit entirely in the alloy. Thicker cladding is made by explosion welding.

Chemical composition of NCF625 cladding and the base

Under JIS G3602 each layer meets the chemistry of its own standard; for weld overlay types the overlay chemistry is agreed between the parties. The cladding table gives the ASTM limits of UNS N06625 for reference, because most export orders are checked against them; a JIS G4902 NCF625 certificate reports the limits of the JIS standard, and a dual-certified heat must meet both.

Inconel 625 (N06625) cladding, ASTM limits for reference

Element N06625, %
Nickel (Ni) 58.0 min
Chromium (Cr) 20.0 – 23.0
Molybdenum (Mo) 8.0 – 10.0
Niobium + tantalum (Nb + Ta) 3.15 – 4.15
Iron (Fe) 5.0 max
Carbon (C) 0.10 max
Manganese (Mn) 0.50 max
Silicon (Si) 0.50 max
Phosphorus (P) 0.015 max
Sulfur (S) 0.015 max
Aluminium (Al) 0.40 max
Titanium (Ti) 0.40 max
Cobalt (Co), if determined 1.0 max

The limits are those of ASTM B443 for UNS N06625. The iron limit of 5.0 % is the figure most often discussed with clad plate, because it is the reference used when judging iron pick-up in weld overlays at clad seams. A JIS G4902 certificate reports the JIS limits for NCF625.

Example base: SGV480 (JIS G3118)

Element SGV480 heat analysis, % (JIS G3118)
C, 6 – 12.5 mm ≤ 0.27
C, over 12.5 – 50 mm ≤ 0.28
C, over 50 – 100 mm ≤ 0.30
C, over 100 – 200 mm ≤ 0.31
Si 0.15 – 0.40
Mn 0.85 – 1.20
P, S Per the JIS G3118 edition ordered

For other bases, such as SB410 or SPV355, the chemistry is that of JIS G3103 or JIS G3115 and is reported on the base mill certificate. Keep the base sulfur low where the plate will be heavily formed, because it helps both bonding and later welding.

Mechanical properties, bend and shear tests

JIS G3602 Table 2 sets the requirements for the clad steel as a product.

Property Rolled, explosion and diffusion clad steel Weld overlay clad steel
Tensile strength Not less than σB = (t1·σB1 + t2·σB2) / (t1 + t2) Same
Elongation Not less than the lower of the base and cladding specified values Same
Bend, 180° Face bend: inside radius per the cladding standard; back bend: per the base standard; never less than 1 × total thickness; no cracks Face bend, inside radius 2 × total thickness; cracks under 3 mm
Shear strength ≥ 200 N/mm² Not specified

In the formula, σB1 is the specified minimum tensile strength of the base, σB2 that of the cladding, and t1 and t2 the base and cladding thicknesses. For class 2 clad steel, for forged or cast bases, or when the purchaser specifies it, the tensile test is made on the base only, and the yield and tensile strength must meet the base standard.

A face bend may be left out when the cladding standard has no bend requirement, and a back bend when the base standard has none. A side bend can replace the face bend; then no crack of 1.6 mm or more is allowed on the outside of the bend.

N06625 cladding strength (ASTM annealed plate, for reference)

Property Inconel 625 (N06625)
Tensile strength 758 MPa min (Grade 1, annealed, hot-rolled plate)
Yield strength (0.2 %) 379 MPa min
Elongation 30 % min
Hardness Not specified in B443

Example base: SGV480

SGV480 property (JIS G3118) Requirement
Yield point or proof stress ≥ 265 N/mm²
Tensile strength 480 – 590 N/mm²
Elongation, 6 – 40 mm, No. 1A test piece ≥ 17 %
Elongation, over 50 mm, No. 10 test piece ≥ 21 %
Delivery As rolled up to 38 mm; normalized over 38 mm

Worked example for class 1, 3 mm NCF625 on 20 mm SGV480, using the reference cladding values above (ASTM values): σB = (20 × 480 + 3 × 758) / 23 = 516 N/mm². The certificate uses the JIS G4902 minimum for NCF625, so confirm the figure against the edition ordered. Elongation must meet the lower of the two specified values. If the design also needs a composite yield value, the same weighting gives about (20 × 265 + 3 × 379) / 23 = 280 N/mm², a planning estimate only. For class 2, the SGV480 alone is tested against 265 N/mm² and 480 to 590 N/mm².

Bonding, ultrasonic inspection and corrosion testing

JIS G3602 clause 7 sets the bonding condition, and clause 12 lists the tests, with the methods taken from JIS G0601, the Japanese standard for testing clad steel. Bond quality is checked by ultrasonic testing over the plate and graded by the extent of unbonded area; the grade and scanning coverage should be stated in the order, especially for tube sheets that will be drilled.

Corrosion tests of the NCF625 layer are not a routine product test, so if the service needs one, name the method, the acceptance and the condition of the samples: as bonded, or after the heat treatment the vessel will receive. For nickel claddings the most common request is a test after simulated PWHT.

NCF625 is much stronger than the base, so flattening after explosion bonding puts more load on the interface than with nickel 200 or stainless. That is one reason we scan every plate after flattening, not before, and report the measured shear values on the certificate.

Clad plate or weld overlay?

On a 625-clad vessel, overlay with ERNiCrMo-3 is kept for nozzles, flange faces and repairs. Each overlay layer picks up iron from the steel, so two or more layers are needed before the surface approaches the 5 % iron limit of wrought 625; an explosion clad plate has no dilution, so 3 mm of cladding is 3 mm of full-chemistry alloy across the whole shell.

Manufacturing method, heat treatment and delivery

JIS G3602 clause 11 covers the manufacturing method. In practice the delivery condition follows the base steel standard, since the base carries the load: SGV480, for example, is as rolled up to 38 mm and normalized above that. The cladding face is delivered as bonded and cleaned, or as agreed.

JIS G3602 NCF625 clad plate is normally delivered as clad and flattened, with the 625 sheet annealed before bonding; a full anneal of the alloy after bonding is impractical with a carbon steel base. If the vessel needs PWHT, qualify the cycle on coupons and consider a corrosion test of the cladding afterwards, since long holds at intermediate temperatures can reduce 625’s ductility.

Keep the nickel face clean before heating

Nickel and its alloys are embrittled by sulfur, phosphorus, lead and other low-melting contaminants picked up at high temperature. Before normalizing, stress relief, hot forming or welding, remove marking crayon, paint, oil and shop dirt from the NCF625 surface, and keep high-sulfur furnace atmospheres away from it. Use sulfur-free markers only.

Dimensions, tolerances and weight

Clause 8 of JIS G3602 sets tolerances for width and length (8.1), thickness (8.2) and flatness (8.3), building on JIS G3193 for hot-rolled plate. The cladding and total thickness tolerances are the ones to confirm at the order stage, because they decide the corrosion allowance actually delivered.

Item What to state in the order
Cladding thickness Nominal, and a minimum if the corrosion allowance must be guaranteed
Base thickness Nominal, per the base steel standard
Width and length Finished size, or size before cutting into discs or head blanks
Flatness Standard, or special flatness for tube sheets
Surface Cladding pickled, ground or polished; base as rolled or blasted

Theoretical weight uses a nominal 8.44 g/cm³ for NCF625 and 7.85 g/cm³ for the carbon steel base. A 3 + 20 mm plate therefore weighs about 3 × 8.44 + 20 × 7.85 = 182.3 kg per square metre, and a 2000 × 6000 mm plate about 2.19 t.

Stock sizes and thickness combinations of JIS G3602 NCF625 clad plate

JIS G3602 NCF625 clad plate is specified by cladding and base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 10 12 Thin shells
2 + 14 16 FGD parts
3 + 16 19 Vessel shells
3 + 20 23 Reactors
3 + 30 33 Heads
4 + 40 44 Thick shells
6 + 60 and over 66 and over Tube sheets
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Welding JIS G3602 NCF625 clad plate

JIS clad steel is welded in the usual clad sequence: weld the carbon steel base first with matching filler, then restore the NCF625 face with nickel alloy filler. Carbon steel filler must not be deposited on the cladding.

  1. Bevel from the base side and set back the cladding at the root as the procedure requires.
  2. Weld the base with low-hydrogen carbon steel filler matched to the base grade.
  3. Back-gouge from the clad side to sound weld metal.
  4. Restore the cladding with ERNiCrMo-3 (AWS A5.14) or ENiCrMo-3 (AWS A5.11), which matches alloy 625, using at least two layers so that the surface layer is not diluted by iron from the steel.
  5. Check the finished clad-side weld visually and by penetrant testing.

ERNiCrMo-3 matches 625 and is also the filler commonly used on other nickel alloy claddings. Keep interpass temperature low and the joint free of sulfur and lead contamination, which crack nickel welds.

Repair welding of the clad steel itself is covered by JIS G3602 clause 14; repaired areas are checked again before release, and the repair is recorded in the report.

Applications of JIS G3602 NCF625 nickel alloy clad steel plate

JIS G3602 NCF625 clad steel plate is used where the medium would pit or crack cheaper claddings and the vessel must still be built economically from carbon steel.

  • Flue gas desulfurization absorbers, ducts and outlet parts.
  • Offshore and sour gas separators.
  • Chloride-bearing chemical reactors.
  • Sea water heat exchangers and tube sheets.
  • Phosphoric and mixed acid equipment.
  • High-temperature corrosive service within the base limits.

Ordering tips

State the medium, chloride level, design temperature and whether PWHT is required. For flue gas parts give panel sizes so large plates can cut seams; for tube sheets give the drilled-zone diameter, so the cladding thickness and the UT grade can be agreed.

Tests, inspection, retests and report

JIS G3602 clause 12 lists the tests, clause 13 the inspection, clause 15 retests, clauses 16 and 17 the product symbol and marking, and clause 18 the report.

Test Requirement for JIS G3602 NCF625
Chemical analysis Cladding and base per their own standards
Tensile Composite (class 1) or base only (class 2), per Table 2
Bend Face and back bends, 180°, per Table 2
Shear ≥ 200 N/mm² for rolled, explosion and diffusion clad steel
Ultrasonic test Bond inspection per JIS G0601, grade as ordered
Dimensions and appearance Clause 8 tolerances; visual check of both surfaces (clause 9)
Corrosion test NCF625 layer, only when ordered; method and acceptance by agreement

The inspection document is issued to JIS G0415 / EN 10204 3.1, or 3.2 with third-party inspection. It reports the clad steel symbol, the NCF625 and base grades and heats, thicknesses and all test results.

Equivalent standards and grades

JIS G3602 sits beside the ASTM and Chinese nickel clad plate standards; the test levels differ, so compare before substituting.

Standard Bond shear requirement Classification
JIS G3602 ≥ 200 N/mm² (not for weld overlay) Method code + class 1 / 2
ASTM A265 / ASME SA-265 ≥ 140 MPa, when specified UT class as ordered
NB/T 47002.2-2019 210 MPa benchmark (GB/T 150.2) Method code + class
Layer JIS UNS EN GB
Cladding NCF625 (JIS G4902) N06625 2.4856 (NiCr22Mo9Nb) NS3306
Base SGV480 (JIS G3118) SA516 Gr.70 (approx.) P355GH (approx.) Q345R (approx.)

For ASME work the nearest product is SA516 Gr.70 + alloy 625 to ASME SA-265. Equivalence is approximate. Check chemistry, strength and test requirements against the design code before substituting.

Why order JIS G3602 NCF625 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China and supplies nickel alloy clad steel to Japanese-standard projects in Asia and beyond. For NCF625 clad plate we can supply alloy 625 certified to JIS G4902 and, when the heat meets both, to ASTM B443 as well.

  • We confirm the method code and class (for example B1 or BR2) and the base grade before production.
  • Cladding to JIS G4902 and base to its JIS standard come with traceable mill certificates.
  • Each plate is ultrasonically tested, and shear and bend results are reported on the certificate.
  • Plates can be cut into tube sheet discs and head blanks.

FAQ

Which standard covers the NCF625 cladding?
NCF625 is a JIS G4902 grade. JIS G3602 takes the cladding chemistry and properties from that standard and adds the clad steel tests: shear, bend, composite tensile and ultrasonic bond inspection.
What tensile strength does 3 + 20 mm NCF625 on SGV480 need?
For class 1, JIS G3602 uses the thickness-weighted average. With SGV480 at 480 N/mm² and the reference NCF625 value of 758 N/mm², that is about 516 N/mm²; confirm with the JIS G4902 minimum. Class 2 is tested on the SGV480 alone.
Is JIS G3602 NCF625 the same as ASTM A265 alloy 625 clad plate?
They are close equivalents, not identical. JIS G3602 requires at least 200 N/mm² shear for rolled, explosion and diffusion types; ASTM A265 requires 140 MPa only when the shear test is specified. The cladding is certified to JIS G4902 rather than ASTM B443, so cite both only with a dual-certified heat.
What is the difference between class 1 and class 2 in JIS G3602?
Class 1 is clad steel designed with the cladding as a strength member, or for special uses such as high temperature or severe forming. Class 2 covers the rest, typically where the cladding is a corrosion allowance. Class 2 is tensile tested on the base only.
What shear strength does JIS G3602 require?
At least 200 N/mm² for rolled, explosion and diffusion clad steel. Weld overlay clad steel has no shear requirement.
What is the HS code for nickel alloy clad steel plate?
Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The code depends on the base steel and width, so confirm with your customs broker.
What should I send for a quotation?
JIS G3602, the type and class (for example B1), NCF625 cladding thickness, base grade and thickness, width, length, quantity, tests beyond the standard and certificate type.

Request a quotation for JIS G3602 NCF625 (Alloy 625) Nickel Alloy Clad Steel Plate

JIS G3602 NCF625 nickel alloy clad steel plate bonds alloy 625 to a JIS base steel such as SGV480 or SB410. The standard classifies it by method code and class 1 or 2, requires at least 200 N/mm² bond shear for rolled, explosion and diffusion types, and sets thickness-weighted tensile, bend and ultrasonic tests.

Send the type and class, thickness pair, base grade, size and quantity to SHH STEEL, or compare other grades under JIS G3602 and on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X