JIS G3602 NCF825 (Alloy 825) Nickel Alloy Clad Steel Plate

JIS G3602 NCF825 nickel alloy clad steel plate bonds alloy 825 (UNS N08825) to a JIS pressure vessel steel such as SGV480 or SB410. JIS G3602 classifies it by method code and class 1 or 2 and requires at least 200 N/mm² bond shear for explosion and rolled types. SHH STEEL produces it in China on the base your order names.
Keywords
JIS G3602 NCF825 clad plate, alloy 825 clad steel plate, NCF825 + SGV480, JIS G3602 nickel clad steel, nickel alloy clad steel plate
Equivalent Grades:
ASTM A265 / ASME SA-265, NB/T 47002.2; NCF825 = alloy 825 / UNS N08825 / 2.4858 (NiCr21Mo) / NS1402
Share:
General Description
Material Specification
Base and Cladding Materials
Chemical Composition
Mechanical Properties
Bonding Condition
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is JIS G3602 NCF825 (alloy 825) nickel alloy clad steel plate?

JIS G3602 NCF825 (alloy 825) nickel alloy clad steel plate is a composite plate in which NCF825 (alloy 825, UNS N08825) to JIS G4902 is metallurgically bonded to a JIS carbon or low-alloy steel base, ordered to JIS G3602 “Nickel and nickel alloy clad steels”. The base, usually a pressure vessel steel such as SGV480, carries the load; the NCF825 face resists the process medium. The standard covers clad steel for pressure vessels, nuclear reactors and storage tanks.

NCF825 is the JIS G4902 designation of alloy 825, the titanium-stabilized iron-nickel-chromium alloy with molybdenum and copper often sold as Incoloy 825. It sits between the stainless steels and the Ni-Cr-Mo alloys: it resists sulfuric and phosphoric acid and chloride stress corrosion cracking at a price well below alloy 625 or C-276.

A typical order reads: JIS G3602 B2, NCF825 3 mm + SGV480 20 mm, 2000 × 6000 mm. That line fixes the method and class, both grades, both thicknesses and the plate size, and it is the format we ask for when quoting.

SHH STEEL can produce JIS G3602 NCF825 clad plate in China, mainly by explosion bonding and explosion-rolling, on the JIS base steel your order names. We work to JIS G3602:2012, confirmed in 2017, and certify each plate to its tests.

JIS G3602 types, classes and symbols

JIS G3602 uses the same classification as the other Japanese clad steel standards: a letter code for the manufacturing method and a number for the class. The method codes below are taken from the standard’s Table 1.

Manufacturing method Class 1 Class 2
Rolled clad steel R1 R2
Explosion-rolled clad steel BR1 BR2
Diffusion-rolled clad steel DR1 DR2
Overlay-rolled clad steel WR1 WR2
Cast-in rolled clad steel ER1 ER2
Explosion clad steel B1 B2
Diffusion clad steel D1 D2
Weld overlay clad steel W1 W2
Class Meaning in JIS G3602
Class 1 (…1) Designed with the cladding included as a strength member, and clad steel for special uses, such as high-temperature service or severe working during fabrication
Class 2 (…2) All other clad steel, for example where the cladding is a corrosion allowance or replaces a lining

The class decides how the plate is tested. Under the Table 2 notes, class 2 clad steel, clad steel on a forged or cast base, and any plate where the purchaser asks for it are tensile tested on the base alone, against the base standard; a full-thickness test can replace that by agreement. Class 1 is tested as a composite against a thickness-weighted strength. The shear test, at least 200 N/mm², applies to rolled, explosion and diffusion clad steel; weld overlay clad steel has no shear requirement.

For NCF825 clad plate, explosion clad (B1 or B2) suits tube sheets and thick plate, and explosion-rolled (BR1 or BR2) the larger, thinner plates for shells and heads. Most 825 clad vessels treat the layer as corrosion allowance, so class 2 is the normal choice; class 1 is kept for hot service, heavy forming or designs that count the cladding.

NCF825 cladding and JIS base steels

JIS G3602 takes the chemistry and properties of each layer from its own product standard (clause 10, materials). Nickel and nickel alloy claddings come from two Japanese standards: JIS H4551 for nickel and nickel alloy plate (the NW designations) and JIS G4902 for corrosion- and heat-resisting superalloy plate (the NCF designations). NCF825 is a JIS G4902 grade.

Base steel standard (cited in JIS G3602) Typical grades Use
JIS G3118, carbon steel plates for pressure vessels for intermediate and moderate temperature SGV480, SGV410, SGV450 Most clad pressure vessels
JIS G3103, carbon and molybdenum steel plates for boilers and pressure vessels SB410, SB450, SB480 Boilers, vessels
JIS G3115, steel plates for pressure vessels SPV355, SPV235, SPV315 Higher-yield vessel shells
JIS G3126, carbon steel plates for low temperature pressure vessels SLA grades Low-temperature service
JIS G4109, Cr-Mo steel plates for boilers and pressure vessels SCMV grades Elevated-temperature service
JIS G3106, rolled steels for welded structure SM400, SM490 Non-pressure tanks and structures

Why NCF825 (Incoloy 825) is used

Alloy 825 contains 38.0 to 46.0 % nickel, 19.5 to 23.5 % chromium, 2.5 to 3.5 % molybdenum, 1.5 to 3.0 % copper, 0.6 to 1.2 % titanium and at least 22 % iron. Nickel gives resistance to chloride stress corrosion cracking; molybdenum and copper give resistance to reducing acids, sulfuric acid in particular; chromium handles oxidizing media such as nitric acid.

Titanium stabilizes the alloy against sensitization, which suits clad plate that must go through the base steel’s heat treatment and later PWHT. In pitting resistance 825 is below 625 and C276, so it is not the first choice for hot seawater or strong chlorides.

Where N08825 cladding performs and where it does not

Medium or condition N08825 cladding
Sulfuric acid, moderate temperature Good; copper and molybdenum help
Phosphoric acid Good
Sour gas with chlorides Good; resists stress cracking
Nitric acid Good
Hot concentrated chlorides Pitting risk; 625 or C276 better
Chloride stress corrosion cracking Highly resistant

Choosing the base

SGV480 and SB410 are the usual bases for JIS clad vessels, with SPV355 where higher yield reduces thickness and SCMV grades where the design temperature needs Cr-Mo steel. When an export project asks for “JIS G3602 NCF825” without naming a base, we confirm the base grade and its standard before quoting, because the base decides the strength, the heat treatment and the welding procedure.

Nickel alloy cladding is expensive, so thickness is chosen carefully. Most vessel shells use 2 to 3 mm of N08825; tube sheets often need more so that tube-to-tubesheet welds sit entirely in the alloy. Thicker cladding is made by explosion welding.

Chemical composition of NCF825 cladding and the base

Under JIS G3602 each layer meets the chemistry of its own standard; for weld overlay types the overlay chemistry is agreed between the parties. The cladding table gives the ASTM limits of UNS N08825 for reference, because most export orders are checked against them; a JIS G4902 NCF825 certificate reports the limits of the JIS standard, and a dual-certified heat must meet both.

Incoloy 825 (N08825) cladding, ASTM limits for reference

Element N08825, %
Nickel (Ni) 38.0 – 46.0
Chromium (Cr) 19.5 – 23.5
Iron (Fe) 22.0 min
Molybdenum (Mo) 2.5 – 3.5
Copper (Cu) 1.5 – 3.0
Titanium (Ti) 0.6 – 1.2
Carbon (C) 0.05 max
Manganese (Mn) 1.0 max
Silicon (Si) 0.5 max
Sulfur (S) 0.03 max
Aluminium (Al) 0.2 max

The limits are those of ASTM B424 for UNS N08825. Note that iron is specified as a minimum: 825 is a nickel-iron-chromium alloy with a large iron content, which is one reason it costs less than 625. A JIS G4902 certificate reports the JIS limits for NCF825.

Example base: SGV480 (JIS G3118)

Element SGV480 heat analysis, % (JIS G3118)
C, 6 – 12.5 mm ≤ 0.27
C, over 12.5 – 50 mm ≤ 0.28
C, over 50 – 100 mm ≤ 0.30
C, over 100 – 200 mm ≤ 0.31
Si 0.15 – 0.40
Mn 0.85 – 1.20
P, S Per the JIS G3118 edition ordered

For other bases, such as SB410 or SPV355, the chemistry is that of JIS G3103 or JIS G3115 and is reported on the base mill certificate. Keep the base sulfur low where the plate will be heavily formed, because it helps both bonding and later welding.

Mechanical properties, bend and shear tests

JIS G3602 Table 2 sets the requirements for the clad steel as a product.

Property Rolled, explosion and diffusion clad steel Weld overlay clad steel
Tensile strength Not less than σB = (t1·σB1 + t2·σB2) / (t1 + t2) Same
Elongation Not less than the lower of the base and cladding specified values Same
Bend, 180° Face bend: inside radius per the cladding standard; back bend: per the base standard; never less than 1 × total thickness; no cracks Face bend, inside radius 2 × total thickness; cracks under 3 mm
Shear strength ≥ 200 N/mm² Not specified

In the formula, σB1 is the specified minimum tensile strength of the base, σB2 that of the cladding, and t1 and t2 the base and cladding thicknesses. For class 2 clad steel, for forged or cast bases, or when the purchaser specifies it, the tensile test is made on the base only, and the yield and tensile strength must meet the base standard.

A face bend may be left out when the cladding standard has no bend requirement, and a back bend when the base standard has none. A side bend can replace the face bend; then no crack of 1.6 mm or more is allowed on the outside of the bend.

N08825 cladding strength (ASTM annealed plate, for reference)

Property Incoloy 825 (N08825)
Tensile strength 586 MPa min (annealed)
Yield strength (0.2 %) 241 MPa min
Elongation 30 % min
Hardness Not specified in B424

Example base: SGV480

SGV480 property (JIS G3118) Requirement
Yield point or proof stress ≥ 265 N/mm²
Tensile strength 480 – 590 N/mm²
Elongation, 6 – 40 mm, No. 1A test piece ≥ 17 %
Elongation, over 50 mm, No. 10 test piece ≥ 21 %
Delivery As rolled up to 38 mm; normalized over 38 mm

Worked example for class 1, 3 mm NCF825 on 20 mm SGV480, using the reference cladding values above (ASTM values): σB = (20 × 480 + 3 × 586) / 23 = 494 N/mm². The certificate uses the JIS G4902 minimum for NCF825, so confirm the figure against the edition ordered. Elongation must meet the lower of the two specified values. If the design also needs a composite yield value, the same weighting gives about (20 × 265 + 3 × 241) / 23 = 262 N/mm², a planning estimate only. For class 2, the SGV480 alone is tested against 265 N/mm² and 480 to 590 N/mm².

Bonding, ultrasonic inspection and corrosion testing

JIS G3602 clause 7 sets the bonding condition, and clause 12 lists the tests, with the methods taken from JIS G0601, the Japanese standard for testing clad steel. Bond quality is checked by ultrasonic testing over the plate and graded by the extent of unbonded area; the grade and scanning coverage should be stated in the order, especially for tube sheets that will be drilled.

Corrosion tests of the NCF825 layer are not a routine product test, so if the service needs one, name the method, the acceptance and the condition of the samples: as bonded, or after the heat treatment the vessel will receive. For nickel claddings the most common request is a test after simulated PWHT.

Alloy 825 is stabilized with titanium, which helps it keep its corrosion resistance after the heat of bonding and later welding. Its strength is close to that of the carbon steel base, so flattening and forming are straightforward; we report the measured shear values on the certificate.

Clad plate or weld overlay?

Matching 825 overlay consumables are uncommon, and many fabricators overlay 825 parts with 625-type filler instead. For large shells, an 825 clad plate gives a uniform, undiluted layer at a lower cost per square metre than multi-layer overlay, and the overlay is kept for nozzles and local repairs.

Manufacturing method, heat treatment and delivery

JIS G3602 clause 11 covers the manufacturing method. In practice the delivery condition follows the base steel standard, since the base carries the load: SGV480, for example, is as rolled up to 38 mm and normalized above that. The cladding face is delivered as bonded and cleaned, or as agreed.

JIS G3602 NCF825 clad plate is commonly delivered as clad and flattened, or stress relieved by agreement, with the 825 sheet annealed before bonding. The titanium-stabilized alloy tolerates the base’s stress relief and PWHT well, which makes 825 a forgiving choice for vessels that need PWHT.

Keep the nickel face clean before heating

Nickel and its alloys are embrittled by sulfur, phosphorus, lead and other low-melting contaminants picked up at high temperature. Before normalizing, stress relief, hot forming or welding, remove marking crayon, paint, oil and shop dirt from the NCF825 surface, and keep high-sulfur furnace atmospheres away from it. Use sulfur-free markers only.

Dimensions, tolerances and weight

Clause 8 of JIS G3602 sets tolerances for width and length (8.1), thickness (8.2) and flatness (8.3), building on JIS G3193 for hot-rolled plate. The cladding and total thickness tolerances are the ones to confirm at the order stage, because they decide the corrosion allowance actually delivered.

Item What to state in the order
Cladding thickness Nominal, and a minimum if the corrosion allowance must be guaranteed
Base thickness Nominal, per the base steel standard
Width and length Finished size, or size before cutting into discs or head blanks
Flatness Standard, or special flatness for tube sheets
Surface Cladding pickled, ground or polished; base as rolled or blasted

Theoretical weight uses a nominal 8.14 g/cm³ for NCF825 and 7.85 g/cm³ for the carbon steel base. A 3 + 20 mm plate therefore weighs about 3 × 8.14 + 20 × 7.85 = 181.4 kg per square metre, and a 2000 × 6000 mm plate about 2.18 t.

Stock sizes and thickness combinations of JIS G3602 NCF825 clad plate

JIS G3602 NCF825 clad plate is specified by cladding and base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 12 14 Thin shells
3 + 14 17 Coolers
3 + 16 19 Separators
3 + 24 27 Columns
4 + 36 40 Heads
5 + 50 55 Thick shells
6 + 60 and over 66 and over Tube sheets
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

Welding JIS G3602 NCF825 clad plate

JIS clad steel is welded in the usual clad sequence: weld the carbon steel base first with matching filler, then restore the NCF825 face with nickel alloy filler. Carbon steel filler must not be deposited on the cladding.

  1. Bevel from the base side and set back the cladding at the root as the procedure requires.
  2. Weld the base with low-hydrogen carbon steel filler matched to the base grade.
  3. Back-gouge from the clad side to sound weld metal.
  4. Restore the cladding with a nickel-base filler qualified for 825, most often ERNiCrMo-3 (625 type), which over-matches 825 in corrosion resistance, using at least two layers so that the surface layer is not diluted by iron from the steel.
  5. Check the finished clad-side weld visually and by penetrant testing.

Matching 825 fillers are less widely stocked; many shops restore 825 cladding with 625-type ERNiCrMo-3, which over-matches it in corrosion resistance. Agree the filler with the end user if sulfuric acid service makes the weld composition important.

Repair welding of the clad steel itself is covered by JIS G3602 clause 14; repaired areas are checked again before release, and the repair is recorded in the report.

Applications of JIS G3602 NCF825 nickel alloy clad steel plate

JIS G3602 NCF825 clad steel plate is used in acid and chloride services where stainless claddings crack or corrode and the Ni-Cr-Mo alloys would cost more than the service needs.

  • Sour gas separators and slug catchers.
  • Sulfuric acid coolers and vessels.
  • Phosphoric acid evaporators.
  • Pickling and acid recovery equipment.
  • Refinery overhead drums with chlorides and acids.
  • Heat exchanger shells and tube sheets.

Ordering tips

State the acid, its concentration and temperature, the chloride level and whether PWHT is required. For sour or sulfuric service, ask for a corrosion test after the heat treatment the vessel will receive and give the condition of the samples in the order.

Tests, inspection, retests and report

JIS G3602 clause 12 lists the tests, clause 13 the inspection, clause 15 retests, clauses 16 and 17 the product symbol and marking, and clause 18 the report.

Test Requirement for JIS G3602 NCF825
Chemical analysis Cladding and base per their own standards
Tensile Composite (class 1) or base only (class 2), per Table 2
Bend Face and back bends, 180°, per Table 2
Shear ≥ 200 N/mm² for rolled, explosion and diffusion clad steel
Ultrasonic test Bond inspection per JIS G0601, grade as ordered
Dimensions and appearance Clause 8 tolerances; visual check of both surfaces (clause 9)
Corrosion test NCF825 layer, only when ordered; method and acceptance by agreement

The inspection document is issued to JIS G0415 / EN 10204 3.1, or 3.2 with third-party inspection. It reports the clad steel symbol, the NCF825 and base grades and heats, thicknesses and all test results.

Equivalent standards and grades

JIS G3602 sits beside the ASTM and Chinese nickel clad plate standards; the test levels differ, so compare before substituting.

Standard Bond shear requirement Classification
JIS G3602 ≥ 200 N/mm² (not for weld overlay) Method code + class 1 / 2
ASTM A265 / ASME SA-265 ≥ 140 MPa, when specified UT class as ordered
NB/T 47002.2-2019 210 MPa benchmark (GB/T 150.2) Method code + class
Layer JIS UNS EN GB
Cladding NCF825 (JIS G4902) N08825 2.4858 (NiCr21Mo) NS1402
Base SGV480 (JIS G3118) SA516 Gr.70 (approx.) P355GH (approx.) Q345R (approx.)

For ASME work the nearest product is SA516 Gr.70 + alloy 825 to ASME SA-265. Equivalence is approximate. Check chemistry, strength and test requirements against the design code before substituting.

Why order JIS G3602 NCF825 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China and supplies nickel alloy clad steel to Japanese-standard projects in Asia and beyond. For NCF825 clad plate we can supply alloy 825 certified to JIS G4902 and, when the heat meets both, to ASTM B424 as well.

  • We confirm the method code and class (for example B1 or BR2) and the base grade before production.
  • Cladding to JIS G4902 and base to its JIS standard come with traceable mill certificates.
  • Each plate is ultrasonically tested, and shear and bend results are reported on the certificate.
  • Plates can be cut into tube sheet discs and head blanks.

FAQ

Which standard covers the NCF825 cladding?
NCF825 is a JIS G4902 grade. JIS G3602 takes the cladding chemistry and properties from that standard and adds the clad steel tests: shear, bend, composite tensile and ultrasonic bond inspection.
What tensile strength does 3 + 20 mm NCF825 on SGV480 need?
For class 1, JIS G3602 uses the thickness-weighted average. With SGV480 at 480 N/mm² and the reference NCF825 value of 586 N/mm², that is about 494 N/mm²; confirm with the JIS G4902 minimum. Class 2 is tested on the SGV480 alone.
Is JIS G3602 NCF825 the same as ASTM A265 alloy 825 clad plate?
They are close equivalents, not identical. JIS G3602 requires at least 200 N/mm² shear for rolled, explosion and diffusion types; ASTM A265 requires 140 MPa only when the shear test is specified. The cladding is certified to JIS G4902 rather than ASTM B424, so cite both only with a dual-certified heat.
What is the difference between class 1 and class 2 in JIS G3602?
Class 1 is clad steel designed with the cladding as a strength member, or for special uses such as high temperature or severe forming. Class 2 covers the rest, typically where the cladding is a corrosion allowance. Class 2 is tensile tested on the base only.
What shear strength does JIS G3602 require?
At least 200 N/mm² for rolled, explosion and diffusion clad steel. Weld overlay clad steel has no shear requirement.
What is the HS code for nickel alloy clad steel plate?
Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The code depends on the base steel and width, so confirm with your customs broker.
What should I send for a quotation?
JIS G3602, the type and class (for example B1), NCF825 cladding thickness, base grade and thickness, width, length, quantity, tests beyond the standard and certificate type.

Request a quotation for JIS G3602 NCF825 (Alloy 825) Nickel Alloy Clad Steel Plate

JIS G3602 NCF825 nickel alloy clad steel plate bonds alloy 825 to a JIS base steel such as SGV480 or SB410. The standard classifies it by method code and class 1 or 2, requires at least 200 N/mm² bond shear for rolled, explosion and diffusion types, and sets thickness-weighted tensile, bend and ultrasonic tests.

Send the type and class, thickness pair, base grade, size and quantity to SHH STEEL, or compare other grades under JIS G3602 and on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X