JIS G 3101 SS400 H-Beam | JIS G 3101 H-Beams - SHH STEEL

JIS G 3101 SS400 H-Beam

JIS G 3101 SS400 H-beam is a general-structure rolled section named for a 400–510 MPa tensile range, not a 400 MPa yield. Minimum yield is 245 MPa up to 16 mm. Sizes follow the JIS G 3192 standard H-section series. SHH STEEL reviews grade, size and certificate requirements before quoting.
Keywords
JIS G 3101 SS400 H-Beam, SS400 H-section, JIS G 3192 H-beam, SS400 200×200, SS400 structural H-beam
Equivalent Grades:
Near-equivalents only, not automatic substitutes: Q235B; S235JR; ASTM A36. SM490 is a JIS G 3106 welded-structure family, not this grade.
Share:
General Description
Material Specification
Available Sizes of SS400 H-Beam
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why Source SS400 H-Beams from SHH STEEL
FAQ
Conclusion

What is JIS G 3101 SS400 H-Beam?

JIS G 3101 SS400 H-beam is a hot-rolled H-section in rolled steel for general structure, grade SS400. The material standard is JIS G 3101. Dimensions, mass and tolerances for the section itself are those of JIS G 3192. The “400” in the grade name is the lower end of the specified tensile range (400–510 N/mm²). It is not a 400 MPa yield. Up to 16 mm, the minimum yield point or proof stress is 245 N/mm², and it steps down as the thickness at the test-piece location increases.

This page is for the rolled H-section. The same JIS G 3101 grade in plate form is listed separately as JIS G 3101 SS400 steel plate. Do not use the plate page as a beam data sheet, and do not treat a Chinese HW/HM/HN designation or a European HEA as if it were a JIS H-section of the same nominal depth.

These beams are filed under JIS G 3101 steel beam profiles in the steel beam profiles category of steel structural profiles. The dimensional standard is identified under JIS G 3192. The usual product is the standard H-section series; constant outside-dimension H-sections and I-beams in JIS G 3192 may be furnished when they are named and certified.

SS400 H-beams are used for building and general industrial framing when the specification names this Japanese general-structure grade. The standard does not specify a Charpy test for SS400. The grade is not a pressure-vessel or nuclear safety material, and it is not a substitute for JIS G 3106 SM490 when a welded-structure grade and a defined impact quality are what the order requires.

Material, Dimensions and Tolerances for SS400 Sections

The order and the inspection certificate should keep material, dimensions and tolerances distinct:

  • JIS G 3101 is the material standard. This article uses heat-analysis and tensile values for SS400 sections from JIS G 3101:2024. The edition named on the order governs acceptance.
  • JIS G 3192 is the dimensional standard for hot-rolled sections. The size table below lists the 53 standard H-sections in JIS G 3192 Table 15, with designations, thicknesses, root radius, area and theoretical mass. Those rows are reference dimensions, not a mill rolling list.

A documented special combination — for example SS400 on a W-shape, or a JIS H-section certified to a different material standard — is only valid if every requirement of each named standard is met. Matching a nominal 200 mm or 8 in depth is not a substitution.

SS400 H-Beam Sizes: JIS G 3192 Standard H-Sections

The table lists the 53 standard H-sections of JIS G 3192 Table 15, from H 100×50×5×7 to H 918×303×19×37. The designation is written H × flange width × web thickness × flange thickness, in millimetres. Actual depth is not always the series name: H 148×100×6×9 belongs to the 150×100 series, and H 194×150×6×9 belongs to the 200×150 series. Within one series the inner depth is constant.

Thickness at the test-piece location, usually the flange, is what sets the SS400 yield. H 200×200×8×12 and H 300×300×10×15 have 12 mm and 15 mm flanges, so both remain in the 245 N/mm² band. H 350×350×12×19 has a 19 mm flange, so the minimum yield is 235 N/mm². These figures are for identification and estimating, not a claim that every row is produced in SS400. Mid-range square and narrow H-sections are the usual enquiry core; rows marked * are identified in Table 15 as other than general-purpose and should be confirmed size by size.

Swipe horizontally to view all dimensions.

Designation (H×B×t1×t2) h (mm) b (mm) t1 (mm) t2 (mm) r (mm) A (cm²) Mass (kg/m)
H 100×50×5×7 100 50 5 7 8 11.85 9.30
H 100×100×6×8 100 100 6 8 8 21.59 16.9
H 125×60×6×8 125 60 6 8 8 16.69 13.1
H 125×125×6.5×9 125 125 6.5 9 8 30.00 23.6
H 150×75×5×7 150 75 5 7 8 17.85 14.0
H 148×100×6×9 148 100 6 9 8 26.35 20.7
H 150×150×7×10 150 150 7 10 8 39.65 31.1
H 175×90×5×8 175 90 5 8 8 22.90 18.0
H 175×175×7.5×11 175 175 7.5 11 13 51.43 40.4
* H 198×99×4.5×7 198 99 4.5 7 8 22.69 17.8
H 200×100×5.5×8 200 100 5.5 8 8 26.67 20.9
H 194×150×6×9 194 150 6 9 8 38.11 29.9
H 200×200×8×12 200 200 8 12 13 63.53 49.9
* H 248×124×5×8 248 124 5 8 8 31.99 25.1
H 250×125×6×9 250 125 6 9 8 36.97 29.0
H 244×175×7×11 244 175 7 11 13 55.49 43.6
H 250×250×9×14 250 250 9 14 13 91.43 71.8
* H 298×149×5.5×8 298 149 5.5 8 13 40.80 32.0
H 300×150×6.5×9 300 150 6.5 9 13 46.78 36.7
H 294×200×8×12 294 200 8 12 13 71.05 55.8
H 300×300×10×15 300 300 10 15 13 118.5 93.0
* H 346×174×6×9 346 174 6 9 13 52.45 41.2
H 350×175×7×11 350 175 7 11 13 62.91 49.4
H 340×250×9×14 340 250 9 14 13 99.53 78.1
H 350×350×12×19 350 350 12 19 13 171.9 135
* H 396×199×7×11 396 199 7 11 13 71.41 56.1
H 400×200×8×13 400 200 8 13 13 83.37 65.4
H 390×300×10×16 390 300 10 16 13 133.3 105
H 400×400×13×21 400 400 13 21 22 218.7 172
* H 414×405×18×28 414 405 18 28 22 295.4 232
* H 428×407×20×35 428 407 20 35 22 360.7 283
* H 458×417×30×50 458 417 30 50 22 528.6 415
* H 498×432×45×70 498 432 45 70 22 770.1 605
* H 446×199×8×12 446 199 8 12 13 82.97 65.1
H 450×200×9×14 450 200 9 14 13 95.43 74.9
H 440×300×11×18 440 300 11 18 13 153.9 121
* H 496×199×9×14 496 199 9 14 13 99.29 77.9
H 500×200×10×16 500 200 10 16 13 112.3 88.2
* H 482×300×11×15 482 300 11 15 13 141.2 111
H 488×300×11×18 488 300 11 18 13 159.2 125
* H 596×199×10×15 596 199 10 15 13 117.8 92.5
H 600×200×11×17 600 200 11 17 13 131.7 103
* H 582×300×12×17 582 300 12 17 13 169.2 133
H 588×300×12×20 588 300 12 20 13 187.2 147
* H 594×302×14×23 594 302 14 23 13 217.1 170
* H 692×300×13×20 692 300 13 20 18 207.5 163
H 700×300×13×24 700 300 13 24 18 231.5 182
* H 792×300×14×22 792 300 14 22 18 239.5 188
H 800×300×14×26 800 300 14 26 18 263.5 207
* H 890×299×15×23 890 299 15 23 18 266.9 210
H 900×300×16×28 900 300 16 28 18 305.8 240
* H 912×302×18×34 912 302 18 34 18 360.1 283
* H 918×303×19×37 918 303 19 37 18 387.4 304

Rows marked * are the 20 sizes that Table 15 identifies as other than general-purpose. The tabulated dimensions are representative; other section sizes may be used by agreement. Constant outside-dimension H-sections (JIS G 3192 Table 16) and I-beams can be reviewed when they are named on the enquiry. Chinese HW, HM and HN names belong to GB/T 11263; European HEA, HEB and IPE names belong to EN 10025-2 practice, not to this table.

SS400 Chemical Composition (JIS G 3101 Heat Analysis)

The figures below are heat-analysis limits for SS400 in JIS G 3101:2024. They should not be copied from SS540, which does have carbon and manganese maxima, or from a Chinese or European 235 MPa table that publishes carbon and manganese limits SS400 does not. They are limits, not typical heat results.

Element Heat analysis, max (mass %) Notes for SS400
C No tabulated maximum The carbon column for SS400 is a dash, not a zero-carbon requirement. Carbon and other unlisted elements may be added as necessary, and if they are added they shall be reported.
Mn No tabulated maximum The manganese column for SS400 is also a dash. Do not copy an SS540 manganese maximum (1.60%) onto an SS400 order.
Si Not a tabulated column JIS G 3101:2024 Table 2 does not list a silicon maximum for SS330, SS400 or SS490.
P 0.050 This is a heat-analysis maximum, not a typical result.
S 0.050 This is a heat-analysis maximum, not a typical result.

SS400 Mechanical Properties: Yield, Tensile, Elongation and Bend

Tensile properties of SS400 sections follow Table 3 of JIS G 3101:2024 (plates, strips, flats and sections). Thickness is that at the test-piece location. Unless otherwise specified, the yield value is the upper yield point (ReH); if no yield point appears, 0.2% proof stress (Rp0.2) is determined. Annex JA, which applies to sections with a leg length under 40 mm, is not used for the standard H-sections in the size table above, whose flange widths are 50 mm or more.

Thickness at the test-piece location (mm) Minimum yield point or proof stress (N/mm²) Tensile strength (N/mm²)
t ≤ 16 245 400–510
16 < t ≤ 40 235 400–510
40 < t ≤ 100 215 400–510
t > 100 205 400–510

Elongation uses the test pieces named in the same table. For No. 4 test pieces on plates thicker than 90 mm, the standard reduces the tabulated elongation by 1 for each 25 mm or fraction of thickness, with a maximum reduction of 3; that reduction is a plate rule and is not extended here to invent a section value.

Thickness (mm) Test piece Minimum elongation (%)
t ≤ 5 No. 5 21
5 < t ≤ 16 No. 1A 17
16 < t ≤ 40 No. 1A 21
40 < t ≤ 50 No. 1A 21
t > 50 No. 4 23

The specified bend is 180° with an inner radius of 1.5 times the thickness, using a No. 1 test piece (a No. 3 piece may be used at 5 mm and under). The bend test may be omitted unless the purchaser specifies it, but the steel still has to satisfy the bendability requirement. JIS G 3101 does not specify a Charpy test for SS400; a toughness value must not be inferred from the grade name. If the specification needs a defined impact test, a JIS G 3106 quality such as SM490B or SM490C, or another standard that actually tables that test, should be nominated.

Delivery Conditions, Inspection and Identification

SS400 sections are commonly supplied as-rolled. The inspection document should show JIS G 3101 and its edition, the grade SS400, the JIS G 3192 size designation, the delivery condition, the heat number, the heat analysis (including any added elements), and the tensile results by thickness. If not otherwise specified at the time of order, the inspection document is a JIS G 0415 inspection certificate 3.1. A toughness result cannot be inferred from an SS400 certificate.

Type 3.2 or nominated third-party attendance can be added when the specification requires it. Identification follows the mill’s marking practice. Standard lengths in JIS G 3192 are in the region of 6–13 m; other lengths are a matter for the rolling programme and the order.

Weldability and Surface Condition of SS400 H-Beams

SS400 is widely welded in general-structure work, but JIS G 3101 does not table a carbon-equivalent limit for the grade. Procedure, thickness and hydrogen control should be set from the certificate analysis and the applicable welding specification, not from an invented CEV figure. This page does not prescribe a procedure or a preheat chart.

The as-rolled surface is mill scale. Blast, paint or galvanizing is an order option. Because silicon is not limited in the SS400 chemistry table, a galvanizing specification should be reviewed against the actual heat analysis if a coating is planned. Cutting, weld-end preparation, forming or coating can be reviewed when that specification is sent with the enquiry. They are not assumed for every size.

JIS G 3192 Shape Tolerances and Theoretical Mass

Dimensional and mass tolerances for these H-sections are those of JIS G 3192, not of JIS G 3101. This article does not reproduce the millimetre tolerance tables; acceptance is against the edition named on the order.

A delivered H 200×200×8×12 will measure close to 200 × 200 × 8 × 12 mm within those tolerances, not as a set of exact advertised millimetres. Out-of-square and web off-centre matter for end-plate connections. Settlement on theoretical or weighed mass should follow the contract.

Applications and Service Limits

SS400 H-beams are used where a Japanese general-structure grade and the JIS H-section series are specified:

  • Building and industrial frames whose specification names SS400 rather than a welded-structure SM grade or a Chinese or European designation.
  • Export packages that compare the grade with Q235B H-beam or with S235JR, provided each line keeps its own material standard and shape system.

It is not specified here for pressure equipment, for nuclear safety-related components, or for structures that actually require a tabulated impact test. Durability comes from the coating or fire-protection system, not from the SS400 designation.

SS400 Compared with Q235B, S235JR and SM490

SS400, Q235B and S235JR are often grouped in a 235 MPa discussion, but they are not interchangeable certificates. SS400 is named for its 400–510 N/mm² tensile range and does not publish carbon or manganese maxima, nor a Charpy test. Q235B is a Chinese 235 MPa grade on the GB/T 11263 shape system. S235JR, whose plate form is listed as EN 10025-2 S235JR steel plate, carries tabulated carbon and manganese and a +20 °C impact test, and it is rolled as European I and H sections.

SM490A and SM490B can use the same JIS H-section series, but they belong to JIS G 3106, with a higher tensile class and, for B and C, specified impact tests. Dual certification requires every requirement of each named standard to be met on the delivered piece.

Near-Equivalents: Not Automatic Substitutes

The comparisons below are for orientation. They are not a licence to substitute one grade for another on a contract or an inspection certificate.

Grade / designation Standard Relationship to SS400 H-beam Caution
Q235B GB/T 700; dimensions GB/T 11263 A common Chinese 235 MPa comparison used in export enquiries, often as HW, HM or HN sections. Q235B has its own chemistry table, including tabulated carbon and manganese limits that SS400 does not publish. The shape names are not JIS designations.
S235JR EN 10025-2; dimensions EN 10365 A 235 MPa European general-structure comparison, usually as HEA, HEB or IPE. S235JR has tabulated carbon, manganese and a +20 °C impact test. SS400 has no Charpy requirement in JIS G 3101.
ASTM A36 ASTM A36/A36M; dimensions ASTM A6 A lower-yield American comparison, usually as W-shapes. A36 has its own chemistry and shape system. It is not an SS400 certificate by another name.
SM490A / SM490B JIS G 3106; dimensions JIS G 3192 Weldable structural grades that can use the same H-section series, at a higher tensile class. They are a different material standard, with tighter phosphorus and sulphur and, for B and C, specified impact tests. They are not a silent upgrade of SS400.

The SM490 H-beam page in this series will be linked here once it is published. Until then, use the live category, plate and Q235B links above, and the published S355JR H-beam page only as a higher-strength European comparison, not as an SS400 equivalent.

Sourcing SS400 H-Beams from SHH STEEL

SHH STEEL supplies SS400 H-beams as an export trading house, coordinating mill production and project procurement. For this grade the useful work is to keep the tensile-named SS400 designation from being read as a 400 MPa yield, to keep JIS G 3192 designations from being replaced by HW or HEA shorthand, and to align the inspection document with the edition named on the order before a rolling programme is committed.

Sections can be sourced from mills that SHH STEEL buys from, including Masteel, Rizhao Steel, Laiwu (Shandong Steel Laiwu) and Tung Ho Steel, among others when the programme matches the order. Those mills do not each roll every JIS H-section in SS400. Mid-range sizes are the usual core; asterisked Table 15 rows and very heavy 400×400 variants are confirmed per line.

The same enquiry can also cover Chinese, American or European designations, provided each line states its material standard, shape standard and size. If cutting, weld-end preparation, forming or a coating system is required, include that specification for review. Export packing and container loading can be arranged to the packing list agreed for the shipment.

SS400 H-Beam FAQs

Does SS400 have a 400 MPa yield?
No. The 400 in the grade name is the lower end of the 400–510 N/mm² tensile range. The minimum yield point or proof stress is 245 N/mm² up to 16 mm, then 235, 215 and 205 N/mm² in the thicker bands.
Does JIS G 3101 specify an impact test for SS400?
No. There is no Charpy requirement for SS400 in JIS G 3101. A toughness value must not be inferred from the grade name. If a defined impact test is required, nominate a standard and quality that actually table it, such as a JIS G 3106 grade.
Are C, Si and Mn limited in SS400?
JIS G 3101:2024 Table 2 gives phosphorus and sulphur maxima of 0.050% for SS400. Carbon and manganese are shown as dashes, not as numerical maxima, and silicon is not a tabulated column for this grade. Elements shown as dashes, and elements not listed, may be added as necessary and shall be reported if they are.
Is H 200×200 the same as HE 200 B or HW 200?
No. H 200×200×8×12 is a JIS G 3192 designation. HE 200 B and HW 200×200 belong to European and Chinese shape systems, with their own depths, thicknesses and tolerances. A shared nominal 200 mm is not a substitution method.
Which standards should appear on the inspection document?
At least JIS G 3101 and its edition, the grade SS400, the JIS G 3192 designation, the delivery condition, heat analysis including any added elements, and tensile results by thickness. If not otherwise specified, the inspection document is a JIS G 0415 inspection certificate 3.1.

Request a Quotation for JIS G 3101 SS400 H-Beam

JIS G 3101 SS400 H-beam is a general-structure section with a 400–510 N/mm² tensile range and 245 N/mm² minimum yield up to 16 mm. Nominate the JIS G 3192 H-section size and the material to JIS G 3101:2024 (or the edition on the order). The table is a reference series, not a rolling list. Send the size list, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X