What is GOST 5520-2017 22K steel plate?
GOST 5520 22K Steel Plate is supplied for welded boilers and pressure vessels under GOST 5520-2017, Rolled non-alloy and alloy steel plates for boilers and pressure vessels. Specifications. The standard is in force, implemented in Russia on 1 October 2018, and replaced GOST 5520-79. This page uses the 2017 edition and its corrected tables, not the withdrawn 1979 tables.
22K extends the carbon-boiler group to 120 mm in Table 1, while 15K through 20K stop at 60 mm. Its elevated-temperature Table 9 includes a value at 320°C but does not specify values at every temperature listed for the other carbon grades.
A complete enquiry identifies the grade, thickness, delivery condition, inspection category and ultrasonic class. A grade name alone does not promise every test in the standard. Category 1 is chemistry-only in the base category matrix; other categories add specific tensile, bend, impact or elevated-temperature requirements.
SHH STEEL supplies this plate within the GOST 5520 range under Boiler & Pressure Vessel Steel Plates. We review the ordered category and delivery condition before quoting production and export requirements.
Material specification for GOST 5520 22K
The following scope and ordering requirements come from the 2017 edition. The thickness range is a standard range, not a stock availability claim.
| Parameter | Detail |
|---|---|
| Standard | GOST 5520-2017; in force; replaced GOST 5520-79 |
| Grade | 22K |
| 2017 chemical classification | Non-alloy (clause 7.1.1.1; Annex A) |
| Table 1 thickness | 4–120 mm |
| Dimensions and tolerances | GOST 19903; state dimensional accuracy and flatness on the order |
| Product form | Hot-rolled plate; plate-mill production or coil rolled and cut into sheets |
| Permitted inspection categories (Table 5) | 1–4, 10, 16, 18–21, 23, 24 |
| Delivery condition | As ordered under clause 7.1.5; see Delivery Conditions below |
| Room-temperature tensile and KCU data | Table 6, subject to the ordered category and thickness |
| V-notch impact data | Table 8, subject to category; KCV in J/cm², not absorbed energy in J |
| Elevated-temperature yield | Table 9 for categories 16–18, 23 and 24; test temperature stated in the order |
| Ultrasonic testing | Each plate; class 1, 2 or 3 under GOST 22727, specified by the purchaser |
| Quality document | GOST 7566 or the inspection-document reference cited by the standard; state required document type |
Chemical composition of GOST 5520-2017 22K
The following ladle-analysis limits are the 22K row of GOST 5520-2017 Table 2. A maximum sign means an upper limit, not a target addition. Values are mass percent.
| Element | Ladle analysis, wt. % |
|---|---|
| C | 0.19–0.26 |
| Si | 0.17–0.40 |
| Mn | 0.70–1.00 |
| S | ≤0.025 |
| P | ≤0.035 |
| Cr | ≤0.30 |
| Ni | ≤0.30 |
| Cu | ≤0.30 |
| Mo | ≤0.08 |
| V | ≤0.05 |
Residual arsenic is limited to 0.08 %. Residual nitrogen is limited to 0.008 %, or 0.012 % for electric-furnace steel. Nitrogen up to 0.012 % is also permitted for other melting routes when the plate passes the required impact test after mechanical ageing, irrespective of the ordered category.
Table 2 permits niobium microalloying up to 0.05 %.
Product-analysis deviations are separately defined in Table 3; they must not be used to widen the ladle-analysis order limits. Elements not listed in Table 2 may not be deliberately added without agreement. Any supplementary chemistry requirement must be written on the order.
Mechanical properties and impact tests for GOST 5520 22K
The 22K data below are transcribed from GOST 5520-2017, not from GOST 19281 or a foreign vessel specification. Table 6 tensile tests are at room temperature, specified as 20°C with a +15/−10°C tolerance. The category matrix determines which characteristics are controlled.
| Thickness (mm) | Yield, min (MPa) | Tensile (MPa) | Elongation, min (%) | KCU at room temperature (J/cm²) | KCU at −40°C (J/cm²) | KCU at −70°C (J/cm²) | KCU after mechanical ageing at room temperature (J/cm²) |
|---|---|---|---|---|---|---|---|
| 4–60 | 265 | 430–590 | 22 | 59 | – | – | 29** |
| >60–120 | 255 | 430–590 | 22 | 59 | – | – | 29** |
Table 6 symbols: “+” means testing for statistical data with results recorded, not a numerical acceptance minimum; “−” means the characteristic is not specified or controlled. “**” values are used only by agreement and must be written on the order. Repeated thickness rows with a “**” tensile band represent alternatives, not cumulative limits.
Clause 7.1.6.2 permits elongation adjustments below 8 mm and above 20 mm: a reduction of 1 percentage point per millimetre below 8 mm, or 0.25 percentage point per millimetre above 20 mm, with the latter reduction capped at 2 points relative to Table 6. Apply the clause to the ordered thickness; the table above retains the printed values.
For the five carbon K grades, clause 7.1.6.2 also permits the upper tensile limit to be increased by 29 MPa relative to Table 6. This permission is separate from the printed base range.
V-notch impact, Table 8. KCV is impact toughness per ligament area in J/cm². It is not an absorbed-energy value in joules, and KCU and KCV are not interchangeable.
| Thickness (mm) | KCV +20°C (J/cm²) | KCV 0°C (J/cm²) | KCV −20°C (J/cm²) | KCV −40°C (J/cm²) |
|---|---|---|---|---|
| 5–120 | 39* | + | + | – |
Table 8 applies through the ordered V-notch categories (19–22 and 24), restricted to categories permitted for the grade in Table 5. “+” is statistical-only; “−” is not specified. A single asterisk is retained from the source, whose note gives a historical non-rejection period ending on 1 January 2022. Do not treat starred values as an unconditional exemption from present acceptance requirements.
Impact testing at room and subzero temperatures is required for plate 12 mm and thicker when the category requires it; below 12 mm it is by purchaser request. For the carbon and Mn-Si grades, aged-impact testing is specified from 7 mm; below 7 mm it is on request with results recorded but not used for rejection. Specimen selection follows clause 9.8: full-size types from 10 mm and reduced-size types from 5 to under 10 mm, with the stated thickness-tolerance exceptions. One impact specimen may be 4.9 J/cm² below the table value. These are not permission to omit the ordered tests.
Elevated-temperature yield, Table 9. The temperature is a test condition, not a maximum service temperature or an allowable design stress.
| Requirement | 200°C | 250°C | 300°C | 320°C | 350°C | 400°C | 450°C | 500°C |
|---|---|---|---|---|---|---|---|---|
| Base requirements | 216 | 206 | 191 | 186 | 176 | – | – | – |
All Table 9 numbers are minimum yield strength in MPa. “*” in this table has a different meaning from Tables 6 and 8: the starred value and its test require agreement and inclusion on the order. “−” means no requirement at that temperature. No interpolation or allowable-stress calculation is supplied.
180° bend, Table 7: 4–120 mm: d = 2a. Here d is mandrel diameter and a is specimen thickness. No tears, cracks or laminations are permitted at the bend.
Delivery conditions for GOST 5520 22K
Clause 7.1.5 supplies plate in the condition stated in the order. The standard lists normalizing, normalizing plus tempering, quenching plus tempering, tempering and annealing, including applicable processing from rolling heat; controlled rolling with or without accelerated cooling; controlled rolling followed by high tempering; and hot-rolled delivery without heat treatment.
This list does not mean that every 22K enquiry should default to one treatment. Select the condition with the vessel designer and mill to meet the ordered category. If the condition is not stated, the manufacturer determines it and records it in the quality document. Category 1 is hot-rolled in the base matrix; heat-treated or thermomechanically processed category 1 plate is an agreement option under clause 7.2.6.
The standard does not prescribe one universal normalizing, tempering or welding temperature for this grade on this page. Request the actual heat-treatment regime when the fabrication code requires it; clause 8.3 allows agreed reporting of that information. Fabrication heat treatments and simulated post-weld heat-treatment tests must be discussed before supply.
Weldability and fabrication heat treatment
GOST 5520-2017 clause 7.1.7 states that weldability is ensured by chemical composition and manufacturing technology. This is not a qualified welding procedure for 22K. Welding consumables, preheat, interpass temperature, heat input and any post-weld heat treatment must follow the qualified procedure and the pressure-equipment design requirements.
Thickness, restraint, hydrogen level and the actual heat chemistry influence cracking risk. Matching a nominal carbon or manganese level is not enough to approve a procedure or substitute another steel.
Where the design needs weld or HAZ toughness at a particular temperature, specify it in the procedure qualification. Base-plate KCU or KCV results do not demonstrate the toughness of a completed weld.
Dimensions, surface quality and inspection
Dimensions, thickness deviations and flatness follow GOST 19903. State plate size, manufacturing accuracy and flatness in the enquiry rather than treating the full Table 1 scope as a warehouse size list.
The standard prohibits cracks, rolled-in surface defects and laminations. Grinding or dressing must not take the plate below its permitted minimum thickness. Surface repair by welding is allowed only within clause 7.1.2.3 limits, with its inspection, thermal-treatment and reporting requirements; specify any project restriction on repair welding at enquiry stage.
Every plate is checked for dimensions, surface and edge quality, and ultrasonically examined. GOST 22727 continuity class 1, 2 or 3 is chosen on the order; there is no single universal class for every GOST 5520 grade. Mechanical specimens are transverse to rolling under clause 9.5 unless longitudinal testing is requested with the permitted acceptance adjustment.
Batch acceptance follows GOST 7566 and clauses 8–9. The quality document records the inspection category, delivery condition, test results and internal-defect examination; additional tests and any repair-weld information are reported where applicable. Heat/plate identification must remain traceable through cutting and shipment.
Applications and service limits of 22K
22K plate is specified for welded boiler drums, pressure-vessel shells, heads and other pressure-retaining fabrications where the design specifies a carbon boiler steel. Suitability for a particular temperature, pressure and wall thickness is established by the design code and ordered tests, not by a generic boiler-plate label.
Room-temperature tensile tests and elevated-temperature yield tests do not themselves establish creep life or an allowable operating temperature. Those limits belong in the engineering design and project material specification.
Edition note. Order GOST 5520-2017 explicitly. GOST 5520-79 is the replaced edition; an older designation or catalogue table is not proof that the current category, chemistry and testing requirements have been met.
Related standard ranges include GB/T 713, EN 10028-2 and ASTM A516. These are routes for a design review, not substitute certificates.
Compare GOST 5520 22K with related boiler grades
The other twelve grades in the GOST 5520 range are linked below so a buyer can compare the specified product, not just its name. They are related, not equivalent. Thickness and category entries are from GOST 5520-2017 Tables 1 and 5.
| Material | Type / purpose | Table 1 thickness | Permitted categories | Substitution limit |
|---|---|---|---|---|
| GOST 5520 22K (this plate) | non-alloy carbon boiler steel | 4–120 mm | 1–4, 10, 16, 18–21, 23, 24 | 2017 edition; select delivery condition and category |
| GOST 5520 15K Steel Plate | non-alloy carbon boiler steel | 4–60 mm | 1–4, 10, 16, 18–21, 23, 24 | Related within GOST 5520; different grade requirements |
| GOST 5520 16K Steel Plate | non-alloy carbon boiler steel | 4–60 mm | 1–4, 10, 16, 18–21, 23, 24 | Related within GOST 5520; different grade requirements |
| GOST 5520 18K Steel Plate | non-alloy carbon boiler steel | 4–60 mm | 1–4, 10, 16, 18–21, 23, 24 | Related within GOST 5520; different grade requirements |
| GOST 5520 20K Steel Plate | non-alloy carbon boiler steel | 4–60 mm | 1–5, 10, 11, 16, 18–21, 23, 24 | Related within GOST 5520; different grade requirements |
| GOST 5520 16GS Steel Plate | manganese-silicon boiler and vessel steel, classified as non-alloy in the 2017 edition | 4–160 mm | 1–24 | Related within GOST 5520; different grade requirements |
| GOST 5520 17GS Steel Plate | manganese-silicon boiler and vessel steel, classified as non-alloy in the 2017 edition | 4–50 mm | 1–6, 10–12, 16, 18–24 | Related within GOST 5520; different grade requirements |
| GOST 5520 17G1S Steel Plate | manganese-silicon boiler and vessel steel, classified as non-alloy in the 2017 edition | 4–50 mm | 1–6, 10–12, 16, 18–24 | Related within GOST 5520; different grade requirements |
| GOST 5520 09G2S Steel Plate | low-carbon manganese-silicon alloy boiler and vessel steel | 4–160 mm | 1–24 | Related within GOST 5520; different grade requirements |
| GOST 5520 10G2S1 Steel Plate | low-carbon manganese-silicon alloy boiler and vessel steel | 4–160 mm | 1–24 | Related within GOST 5520; different grade requirements |
| GOST 5520 10Kh2M Steel Plate | chromium-molybdenum alloy boiler and vessel steel | 8–50 mm | 2–3, 16, 18–20, 23, 24 | Related within GOST 5520; different grade requirements |
| GOST 5520 12KhM Steel Plate | chromium-molybdenum alloy boiler and vessel steel | 4–160 mm | 2–3, 16, 18–20, 23, 24 | Related within GOST 5520; different grade requirements |
| GOST 5520 12Kh1MF Steel Plate | chromium-molybdenum-vanadium alloy boiler and vessel steel | 4–50 mm | 2–3, 16, 18–20, 23, 24 | Related within GOST 5520; different grade requirements |
Equivalent grades and related products — not equivalent
No formal equivalence has been verified for the products below. They are related, not equivalent, and are linked for a purchasing/design comparison only. A cross-reference chart cannot replace review of the two complete specifications.
| Country / region | Standard | Grade / product | Relationship | Caveat |
|---|---|---|---|---|
| China | GB/T 713 | GB/T 713 Q245R Steel Plate | Related boiler/vessel plate family; not equivalent | Verify chemistry, thickness, delivery, impact, elevated-temperature tests and design-code approval |
| Europe | EN 10028-2 | EN 10028-2 P265GH Steel Plate | Related boiler/vessel plate family; not equivalent | Verify chemistry, thickness, delivery, impact, elevated-temperature tests and design-code approval |
A similar tensile class or intended use does not establish equal impact testing, delivery condition or elevated-temperature acceptance. Confirm the project design-code route and all supplementary requirements before substitution.
Why choose SHH STEEL for 22K plate
- SHH STEEL produces and exports 22K boiler and pressure-vessel plate to the ordered specification
- We check the 4–120 mm Table 1 scope and ordered category rather than quote one generic 4–160 mm range for every grade
- The quotation separates delivery condition, ultrasonic class and category-specific testing
- We keep GOST 5520-2017 data separate from the replaced edition and from foreign and structural standards
- We review traceability, inspection documents, cutting and export requirements before confirming the order
How to enquire for GOST 5520 22K plate
Send the drawing or material schedule with the following details. Production feasibility, dimensions, documentation and delivery are confirmed against the enquiry.
| Item | What to specify |
|---|---|
| Edition and grade | GOST 5520-2017 22K; no assumed dual certification |
| Dimensions and quantity | Thickness, width, length and tonnage; Table 1 range 4–120 mm |
| Delivery condition | State the required processing condition under clause 7.1.5 |
| Inspection category | Choose from 1–4, 10, 16, 18–21, 23, 24 under Table 5; do not leave the required tests implicit |
| Impact tests | KCU and/or KCV; test temperature, thickness applicability, mechanical ageing and any agreed minima |
| Elevated-temperature yield | Test temperature for the applicable category; identify any agreed Table 9 starred values |
| Ultrasonic examination | GOST 22727 class 1, 2 or 3 as ordered; any supplementary acceptance criteria |
| Fabrication and documentation | PWHT or simulated PWHT requirements, repair-weld restrictions, quality-document type and traceability |
| Supplementary scope | If ordering outside the Table 1 grade thickness range, invoke clause 7.2.5 and agree mechanical and bend requirements; do not extrapolate the tables |
FAQ
-
Is GOST 5520-2017 current for 22K?
- Yes. The 2017 standard is in force and replaced GOST 5520-79. In Russia it was implemented on 1 October 2018. State the 2017 edition and the required category on the order.
-
What thickness range does GOST 5520 specify for 22K?
- Table 1 gives 4–120 mm. This is the grade-specific standard scope, not a stock promise. A different thickness within the overall standard scope needs agreement under clause 7.2.5, including mechanical and bend requirements.
-
Is every 22K plate normalized?
- No. Clause 7.1.5 allows several delivery routes. The ordered condition and category govern supply; if the condition is omitted, the manufacturer determines it and records it in the quality document. Do not assume normalized or QT delivery from the grade name.
-
Does 22K always have a guaranteed subzero Charpy value?
- No. Impact testing depends on the ordered category, thickness, notch type and temperature. KCU and KCV are reported as J/cm² in this standard, not simply absorbed energy in J. Statistical-only entries are not numerical acceptance minima.
-
What should a quotation enquiry include?
- GOST 5520-2017 22K, plate dimensions and quantity, delivery condition, inspection category, impact and elevated-temperature test requirements, ultrasonic class, fabrication heat-treatment requirements and the inspection document.
Request a quotation for GOST 5520 22K plate
Contact SHH STEEL for a quotation for GOST 5520-2017 22K boiler and pressure-vessel plate. Send thickness, width, length, quantity, destination and the project material specification.
Specify the delivery condition and inspection category, required KCU/KCV temperatures and acceptance criteria, any elevated-temperature yield test, and the GOST 22727 ultrasonic class. Include PWHT or simulated PWHT, supplementary testing and the quality-document requirement.
If a related grade or another standard is being considered, send the design requirements for review. We do not assume interchangeability or dual certification from a grade comparison alone.
Contact: admin@steelspecs.com