GOST 14637 St3Gsp Steel Plate | St3Gsp Mn Killed Carbon Steel Plate | GOST 14637 Steel - SHH STEEL

GOST 14637 St3Gsp Steel Plate | St3Gsp Mn Killed Carbon Steel Plate

GOST 14637 St3Gsp (Ст3Гсп) steel plate is a manganese killed (Гсп) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026: it was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89. SHH STEEL produces and exports this manganese killed grade to the ordered 2024 requirements.
Grade
St3Gsp
Standard
GOST 14637-2024
Deoxidation
Mn killed (Гсп)
Categories (Table 1)
3–7 (not 1–2)
Tensile strength (Table 2)
390–570 N/mm²
Delivery (clause 7.1.6)
Cats 3–5 & 7: HR, TM or HT; cat 6: TM or HT only
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of GOST 14637 St3Gsp Steel Plate

GOST 14637 St3Gsp Steel Plate is a manganese killed (Гсп) general-quality nonalloyed plate grade under GOST 14637-2024, Rolled plates from nonalloyed steel of general quality. Specifications. The 2024 edition is the current standard as of 12 November 2026. It was introduced as a national standard of the Russian Federation on 1 March 2025, with the right of early application, and it replaces GOST 14637-89.

St3Gsp is listed in clause 6.1. The Gsp ending marks a manganese (G) killed steel in the St3 class. It has its own Table 2 row: tensile strength 390–570 N/mm²; yield 255 N/mm² (≤20 mm) and 245 N/mm² (>20–40 mm), with the two thicker yield bands marked “+”; elongation 23 % (≤20 mm) and 24 % (>20–40 mm), with the thicker elongation band marked “+”. A plus sign in Table 2 means the characteristic is determined for statistical data and is stated in the quality document; it is not a specified minimum. Do not replace those plus signs with numbers. GOST 14637 St3Gps Steel Plate is the manganese semi-killed counterpart (tensile 370–490 N/mm², with yield and elongation shared with GOST 14637 St3ps Steel Plate and GOST 14637 St3sp Steel Plate). In Table 1, St3Gsp is listed in categories 3–7 only. Categories 1 and 2 are not listed. Every listed category specifies chemical-composition control and includes a Table 4 impact test. State the category on the order.

SHH STEEL supplies this plate in the GOST 14637 range. We review the ordered category, delivery condition and manganese designation, deoxidation, category and statistical Table 2 cells before quoting production and export requirements.

GOST 14637 St3Gsp Steel Plate Material Specification

The applicable product standard for this page is GOST 14637-2024. The official English title is Rolled plates from nonalloyed steel of general quality. Specifications. Orders should state that edition, the grade St3Gsp, the category, dimensions, quantity and any agreed options. A grade name without an edition is incomplete. The thickness and width figures below are the standard scope, not a stock promise.

Parameter Detail
Standard GOST 14637-2024; in force from 1 March 2025; replaces GOST 14637-89
Official English title Rolled plates from nonalloyed steel of general quality Specifications
Grade St3Gsp
Deoxidation Manganese killed (Гсп), as marked by the designation
Scope, sheets Thickness 4 to 160 mm inclusive; width 500 mm and more
Scope, coils Thickness 4 to 25 mm
Dimensions and tolerances Remaining assortment requirements follow GOST 19903; state thickness accuracy and flatness on the order
Permitted inspection categories 3–7 only (Table 1). Categories 1 and 2 are not listed. Category 6 uses Table 3 tensile properties and a different Table 5 bend row, and is delivered thermomechanically treated or heat-treated
Chemical composition Shall conform to GOST 380 (clause 7.1.1.1). Every listed category (3–7) specifies chemical-composition control. The G in the designation marks a manganese variant of the St3 class under GOST 380; those manganese limits are not tabulated on this page. Clause 7.1.1.3 is not written for this grade
Tensile properties Table 2 for categories 3–5 and 7 (390–570 N/mm²); Table 3 for category 6
Yield strength σT Table 2 for categories 3–5 and 7: ≥255 / ≥245 N/mm² in the two thinner bands; the two thicker bands are determined for statistical data (+), not specified minima. Table 3 for category 6. See Mechanical Properties
180° bend Table 5; see Mechanical Properties
Impact toughness Every listed category (3–7): Table 4, in J/cm². Categories 1 and 2 are not listed
Delivery condition Clause 7.1.6, for the categories listed for this grade: categories 3–5 and 7 without heat treatment (hot-rolled), or thermomechanically treated, or heat-treated; category 6 thermomechanically treated or heat-treated only. Categories 1 and 2 are not listed
Ultrasonic testing By agreement, to a class of GOST 22727; class and volume are not implied by the grade
Acceptance, marking and packaging GOST 7566, with the additions in the 2024 standard

GOST 14637 is a general-quality nonalloyed plate standard. It is not a boiler or pressure-vessel plate standard, and it is not a quality carbon structural plate standard. Do not copy figures from those systems onto a GOST 14637 order.

GOST 14637 St3Gsp Steel Plate Chemical Composition

Clause 7.1.1.1 of GOST 14637-2024 requires the chemical composition of the steel by ladle analysis of the ladle sample, and the permissible deviations in the finished product, to conform to GOST 380. This page does not tabulate GOST 380 heat-analysis limits. Confirm every chemistry cell against the applicable official GOST 380 table. This page is not a substitute for that table.

In Table 1, every category listed for this grade (categories 3–7) specifies chemical-composition control. Categories 1 and 2 are not listed, so a delivery without chemistry control is not a listed option. In every listed category, ladle analysis and product deviations shall conform to GOST 380.

The G in the designation marks a manganese (G) variant of the St3 class under GOST 380, relative to GOST 14637 St3sp Steel Plate (killed, without the G). This page does not tabulate those manganese limits, and a manganese designation is not interchangeability with St3sp or with GOST 14637 St3Gps Steel Plate. Confirm the official GOST 380 cells for this grade.

Clause 7.1.1.2 permits manufacture without a lower limit on carbon and manganese, except for plate intended for shipbuilding, wagon-building or welded cylinders, provided the mechanical properties of this standard are met. State that option on the order if it is required.

On purchaser request, clause 7.1.1.4 tightens sulphur and phosphorus for categories 1–5 to S not more than 0.040 % and P not more than 0.030 %. For this grade, categories 1 and 2 are not listed; the request applies when a listed category in that group (categories 3–5) is ordered. For categories 6 and 7, each of these elements shall not exceed 0.025 %. If the tighter request limits are required, state them on the order.

Clause 7.1.1.3, which allows a stated reduction of a carbon or manganese lower limit at thickness up to 10 mm for Ст3кп, Ст3пс and Ст3сп, is not written for St3Gsp. Do not apply that option to this grade.

For subsequent hot-dip galvanizing, clause 7.1.1.5 allows agreed silicon classes. Classes B (silicon 0.14 % to 0.25 %) and D (silicon 0.25 % to 0.35 %) are the classes written for killed (sp) steel. Class A is written for rimmed (kp) steel and is not the class for this killed grade. Galvanizing class is an agreed option, not a default.

A maximum sign is an upper limit, not a target addition. Product-analysis deviations belonging to GOST 380 must not be used to widen ladle-analysis order limits. Numeric GOST 380 element ranges are not tabulated on this page.

GOST 14637 St3Gsp Steel Plate Mechanical Properties

Clause 7.1.7.1 requires the tensile properties of plate in categories 1–5 and 7 to meet Table 2. For this grade, categories 1 and 2 are not listed; the Table 2 values below apply to the listed categories 3–5 and 7. Units are N/mm² for strength (the unit used in the 2024 tables) and % for elongation δ5. Table 2 heading is “not less than or within limits.”

Property Thickness Requirement (Table 2)
Tensile strength σB, N/mm² All thicknesses in the 2024 scope 390–570
Yield strength σT, N/mm² ≤20 mm ≥255
Yield strength σT, N/mm² >20 mm to 40 mm inclusive ≥245
Yield strength σT, N/mm² >40 mm to 100 mm inclusive Determined for statistical data (+)
Yield strength σT, N/mm² >100 mm Determined for statistical data (+)
Elongation δ5, % ≤20 mm ≥23
Elongation δ5, % >20 mm to 40 mm inclusive ≥24
Elongation δ5, % >40 mm Determined for statistical data (+)

This is the Table 2 row that belongs to St3Gsp alone. Tensile strength is 390–570 N/mm². Yield is specified as a minimum only in the two thinner bands (≥255 N/mm² up to 20 mm, ≥245 N/mm² over 20 mm to 40 mm inclusive). In the bands over 40 mm to 100 mm inclusive and over 100 mm, Table 2 marks yield with a plus sign: the characteristic is determined for statistical data and is stated in the quality document; it is not a specified minimum. Elongation is ≥23 % up to 20 mm and ≥24 % over 20 mm to 40 mm inclusive — the middle band is higher than the thinner band, as written in the official cell — and is marked “+” for thickness over 40 mm. Do not replace a plus sign with a number, and do not treat a statistical result as a design minimum. GOST 14637 St3Gps Steel Plate has a different tensile-strength cell (370–490 N/mm²) and does not share this row. Do not take yield or tensile values from another product standard.

Table 2 footnotes that apply when the corresponding cell is a specified value include the following. For coil plate of thickness over 12 mm to 25 mm inclusive, the mechanical-property norms are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. The upper tensile-strength limit may be increased by not more than 50 N/mm² while the other mechanical-property norms are observed, and by agreement with the purchaser without limiting the upper bound. By agreement, for thickness over 20 mm, a specified yield value may be reduced by 10 N/mm²; for this grade that reduction applies where Table 2 states a number (the >20–40 mm band), not where the cell is a plus sign. Table 2 also permits a stated reduction of elongation for thinner plate: for thickness up to 8 mm inclusive, by 1 % absolute for each millimetre of thickness reduction; for thickness over 8 mm, by 1 % absolute. Confirm the application of this footnote against the official table when thin plate is ordered.

By agreement between the manufacturer and the purchaser, plate of St3Gps and St3Gsp may be supplied to Table 2 with a tensile-strength range of 390 to 570 N/mm² inclusive. For St3Gsp that span is the same as the Table 2 cell. State the agreement on the order if it is to be recorded as an agreed supply condition.

For category 6 only, clause 7.1.7.2 requires tensile properties to meet Table 3, not Table 2. Table 3 is not grade-specific. Values are minima:

Thickness Tensile strength σB, N/mm² Yield strength σT, N/mm² Elongation δ5, %
Up to 40 mm inclusive ≥430 ≥295 ≥16
>40 mm Determined for statistical data (+) Determined for statistical data (+) Determined for statistical data (+)

A plus sign in Table 3 means the characteristic is determined for statistical data and is stated in the quality document. The same two-year optional-norm footnote for coil plate of thickness over 12 mm to 25 mm inclusive applies. Category 6 is delivered in the thermomechanically treated or heat-treated condition (clause 7.1.6).

Clause 7.1.8 requires the plate to withstand a 180° cold bend on a mandrel of the diameter in Table 5. At the bend there shall be no fracture, delamination or cracks. The 1.5a / 2.5a / 2.5a diameters apply except when category 6 is ordered:

Property Thickness (a = plate thickness) Requirement (Table 5)
180° cold bend, mandrel diameter d ≤20 mm d = 1.5a
180° cold bend, mandrel diameter d >20 mm to 40 mm inclusive d = 2.5a
180° cold bend, mandrel diameter d >40 mm d = 2.5a

For category 6 of St3ps, St3sp, St3Gps and St3Gsp, Table 5 prescribes larger mandrel diameters. Those diameters apply only when category 6 is ordered:

Property (category 6) Thickness (a = plate thickness) Requirement (Table 5)
180° cold bend, mandrel diameter d ≤20 mm d = 4a
180° cold bend, mandrel diameter d >20 mm to 40 mm inclusive d = 5a
180° cold bend, mandrel diameter d >40 mm d = 5a*

The asterisk on d = 5a for thickness over 40 mm in the category-6 row means the 180° bend result is optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document.

Clause 7.1.7.3 requires impact tests of categories 3–7 to meet Table 4. St3Gsp is listed in all of those categories, and is not listed in categories 1 and 2. Every listed category for this grade therefore includes a Table 4 impact test. Table 4 gives values “in accordance with Table 1”; the figures below are the Table 4 cells for categories 3–7. Units are J/cm², not less than.

Category 3 (KCU at +20 °C), J/cm², not less than:

Thickness KCU at +20 °C, J/cm² (Table 4, category 3)
4.0 to 10.0 mm inclusive ≥78
>10.0 to 30.0 mm inclusive ≥69
>30.0 to 40.0 mm inclusive ≥49
>40.0 to 60.0 mm inclusive ≥49*
>60.0 mm Determined for statistical data (+)

Category 4 (KCU at −20 °C), J/cm², not less than:

Thickness KCU at −20 °C, J/cm²
4.0 to 10.0 mm inclusive ≥39
>10.0 to 30.0 mm inclusive ≥29
>30.0 to 40.0 mm inclusive ≥29*
>40.0 to 60.0 mm inclusive ≥29*
>60.0 mm Determined for statistical data (+)

Category 5 (KCU at −20 °C, KCU after mechanical aging, and KCV at +20 °C), J/cm², not less than:

Thickness KCU at −20 °C KCU after mechanical aging KCV at +20 °C
4.0 to 10.0 mm inclusive ≥39 ≥39 ≥34
>10.0 to 20.0 mm inclusive ≥29 ≥29 ≥34
>20.0 to 30.0 mm inclusive ≥29 ≥29 ≥34*
>30.0 to 40.0 mm inclusive ≥29* ≥29 ≥34*
>40.0 to 60.0 mm inclusive ≥29* ≥29* ≥29*
>60.0 mm + + +

Category 6 (KCU at −40 °C, KCU after mechanical aging, and KCV at 0 °C), J/cm², not less than:

Thickness KCU at −40 °C KCU after mechanical aging KCV at 0 °C
4.0 to 10.0 mm inclusive ≥39 ≥39 ≥34
>10.0 to 20.0 mm inclusive ≥39 ≥29 ≥30
>20.0 to 40.0 mm inclusive ≥39 ≥29 ≥29*
>40.0 to 60.0 mm inclusive ≥39* ≥29* ≥29*
>60.0 mm + + +

Category 7 (KCU at −40 °C, KCU after mechanical aging, and KCV at −20 °C), J/cm², not less than:

Thickness KCU at −40 °C KCU after mechanical aging KCV at −20 °C
4.0 to 10.0 mm inclusive ≥39 ≥29 ≥34*
>10.0 to 40.0 mm inclusive ≥39 ≥29 ≥34*
>40.0 to 60.0 mm inclusive ≥39* ≥29* ≥29*
>60.0 mm + + +

Units are joules per square centimetre (J/cm²), not absorbed energy in joules. A plus sign means the value is determined for statistical data and is stated in the quality document; this page does not replace a plus with a number. Values marked with an asterisk are optional for two years from the date of introduction of the 2024 standard (1 March 2025); results are stated in the quality document. On one specimen, a 30 % reduction of the impact value is allowed provided the average of the test results is not below the Table 4 norm; the average is stated in the quality document. For coil plate of thickness over 12 mm to 25 mm inclusive, the impact norms are likewise optional for those two years. On purchaser request, impact work in joules may be determined instead of impact toughness, with limit values agreed between the manufacturer and the purchaser.

Table 1 footnote 4, which requires manufacture by agreement for categories 2 and 3 of St3ps and St3sp at thickness 5 mm and more (except plate intended for tubes), does not name St3Gsp. Do not treat that footnote as a condition written for this grade. For category 5 plate intended for tubes, confirm any additional impact-test wording against the official table.

GOST 14637 St3Gsp Steel Plate Delivery Conditions

Under clause 7.1.6, plate of categories 1–5 and 7 is manufactured without heat treatment (in the hot-rolled condition), or in the thermomechanically treated condition, or in the heat-treated condition. Category 6 is manufactured in the thermomechanically treated or heat-treated condition only. State the required delivery condition on the order. If the condition is omitted, do not assume a heat-treated or thermomechanically treated delivery from the grade name alone; for the categories in the 1–5 and 7 group that are listed for this grade, the manufacturer may supply the plate hot-rolled. Record the actual condition on the quality document.

St3Gsp may be ordered in categories 3–7 only. Categories 1 and 2 are not listed for this grade in Table 1. State the category on the order. There is no listed chemistry-free, impact-free category-1 option. Category 6 is manufactured in the thermomechanically treated or heat-treated condition only, and its tensile properties follow Table 3 rather than Table 2. Every listed category adds the corresponding Table 4 impact test. A usual hot-rolled delivery is not a substitute for an agreed thermomechanical or heat-treatment condition when the project requires one, and is not available as a listed category-1 or category-2 supply for this grade.

GOST 14637 St3Gsp Steel Plate Weldability

On purchaser request, clause 7.1.2 allows plate to be supplied with a weldability guarantee, designated in the standard as GS. That guarantee is ensured by limiting the ladle-analysis carbon content to not more than 0.22 %. If a weldability guarantee is required, state it on the order. The designation alone does not include it.

This page does not give preheat, interpass, heat-input or post-weld heat-treatment figures. The fabricator is responsible for welding-procedure qualification, consumable selection, preheat and any post-weld heat treatment required by the project specification. Do not take those figures from another standard or from a handbook and apply them as GOST 14637 rules.

St3Gsp is a manganese killed steel. The G designation and a higher Table 2 tensile-strength cell do not make this grade an automatic welding substitute for GOST 14637 St3sp Steel Plate, GOST 14637 St3Gps Steel Plate or the other St3 plates. Do not assume that a procedure qualified on those grades is valid for this grade without qualification. Because official GOST 380 chemistry limits — including the manganese cells for this designation — are not tabulated on this page, do not assume that ladle carbon is already at or below 0.22 %. If the weldability guarantee is required, order it and confirm the carbon restriction against the official texts.

GOST 14637 St3Gsp Steel Plate Tolerances

Remaining assortment requirements — dimensions, shape and permissible deviations beyond the thickness and width scope in clause 6.2.1 — follow GOST 19903. State the required thickness-accuracy class, edge condition and, for plate supplied as sheets, the flatness class on the order. This page does not tabulate numerical deviation limits from GOST 19903.

Surface quality is specified in clause 7.1.3 of the 2024 standard. Defects of the types listed there are not permitted. Dressing is allowed within the depth and area limits stated in that clause; confirm those limits against the official text. Delamination on ends and on untrimmed edges is not permitted.

Ultrasonic testing is not a default requirement. By agreement, clause 7.1.9 allows plate in sheets to be supplied with ultrasonic testing to a class of GOST 22727. The continuity class and the test volume are not implied by the grade or the category; state them on the order if they are required.

GOST 14637 St3Gsp Steel Plate Applications and service limits

GOST 14637-2024 is a general-quality nonalloyed plate specification. Typical uses are structural and general fabrication where the ordered category, thickness and delivery condition of this grade meet the project specification. This page does not assign a service temperature, a pressure rating or a code-allowed stress from the grade name. The purchaser and the designer remain responsible for fitness for the intended duty.

St3Gsp is listed only in categories 3–7, so every listed supply includes chemical-composition control and a Table 4 impact test. For thicknesses over 40 mm, Table 2 does not specify a yield minimum or an elongation minimum; those cells are determined for statistical data (+). Do not treat a statistical result as a specified design minimum, and do not assume a yield value from GOST 14637 St3sp Steel Plate or GOST 14637 St3Gps Steel Plate for those bands. Table 4 states test temperatures and impact values in J/cm², not an allowable operating temperature. The manganese (G) killed designation is a chemistry-class and deoxidation mark, not a weathering or high-strength grade family of its own. This grade is not a boiler or pressure-vessel plate and is not a quality carbon structural plate.

Compare St3Gsp with related GOST 14637 grades

The figures in the table below are from GOST 14637-2024 Table 2 (and the Table 1 category lists). They compare grades inside this standard. A shared carbon class, a shared yield cell or a nearby tensile-strength range is not interchangeability.

Grade Table 2 tensile σB, N/mm² Yield σT, ≤20 mm Elongation δ5, ≤20 mm Table 1 categories
GOST 14637 St3kp Steel Plate 360–460 ≥235 ≥27 1–3
GOST 14637 St3ps Steel Plate 370–480 ≥245 ≥26 1–7
GOST 14637 St3sp Steel Plate 370–480 ≥245 ≥26 1–7
GOST 14637 St3Gps Steel Plate 370–490 ≥245 ≥26 3–7
GOST 14637 St3Gsp Steel Plate (this page) 390–570 ≥255 ≥23 3–7

St3Gsp is the manganese killed St3 grade and the only St3 row in Table 2 with a 390–570 N/mm² tensile-strength cell and with plus signs in the thicker yield and elongation bands. GOST 14637 St3Gps Steel Plate is the manganese semi-killed counterpart (370–490 N/mm², specified yield in every thickness band). GOST 14637 St3sp Steel Plate and GOST 14637 St3ps Steel Plate share a lower tensile-strength cell (370–480 N/mm²) and are listed in categories 1–7; this grade is listed only in categories 3–7. Do not fill this grade’s plus-sign cells from those other rows. A manganese (G) mark or a shared St3 class is not interchangeability.

Purchasers commonly compare the St3 class with GB/T 700 Q235B, EN 10025-2 S235JR and JIS G3101 SS400. A common comparison is not an equivalent. Those grades belong to other product standards, with their own chemistry, tensile, impact and delivery rules. See also the GB/T 700 hub, the EN 10025-2 hub and the JIS G3101 hub. Do not copy a yield, impact or chemistry figure from those pages onto a GOST 14637 order.

GOST 14637 St3Gsp Steel Plate Equivalent Material Grade

The entries below are commonly compared designations, not equivalent grades. GOST 14637-2024 does not publish a one-to-one equivalent-grade table for this designation. A comparable tensile class in another standard is not a substitute: chemistry, deoxidation, impact category and delivery condition must each be checked against the official texts.

Standard Country-Region Equivalent Grade Note
GB/T 700 China GB/T 700 Q235B Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.
EN 10025-2 Europe EN 10025-2 S235JR Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.
JIS G3101 Japan JIS G3101 SS400 Commonly compared with this GOST 14637 grade; not an equivalent. Confirm chemistry, tensile, impact and delivery against each official standard; do not copy figures across.

If a project specification names one of those other grades, order that specification. If it names St3Gsp under GOST 14637-2024, order this grade and the required category. Do not treat a cross-reference as a certified equivalent.

Why choose Us

SHH STEEL produces and exports GOST 14637 plate, including St3Gsp. We review the manganese killed designation, the 390–570 N/mm² Table 2 cell, the statistical (+) yield and elongation bands over 40 mm, and the listing in categories 3–7 only before production, and we state the actual results on the quality document. We do not treat a shared Table 2 cell or a commonly compared foreign grade as a substitute for the ordered designation.

Orders are accepted against GOST 14637-2024. Enquiry details should include grade, category, thickness, width, length or coil mass, quantity, delivery condition and any agreed options (weldability guarantee, galvanizing class, tighter sulphur and phosphorus, ultrasonic class). See the GOST 14637 hub for the product family.

Our Service

Supply covers production to the ordered 2024 requirements, mill documentation, and export packing and shipment. Quality documents record the actual ladle analysis, tensile results and, where the category requires them, impact results, including any characteristic that Table 2, Table 3 or Table 4 marks as determined for statistical data. Ultrasonic testing, a weldability guarantee and a galvanizing class are supplied when they are agreed on the order, not by default.

To enquire, state GOST 14637-2024, grade St3Gsp, the Table 1 category, dimensions, quantity and the required options. SHH STEEL will confirm manufacturability and the inspection plan against that order. This page is a product description; the official standard and the quality document govern acceptance.

FAQ

What is GOST 14637 St3Gsp steel plate?

St3Gsp (Ст3Гсп) is the manganese killed (Гсп) St3 grade under GOST 14637-2024. The G in the designation marks a manganese variant of the St3 class under GOST 380; those manganese limits are not tabulated on this page. It has its own Table 2 row: tensile strength 390–570 N/mm², with statistical (+) yield and elongation cells in the thicker bands. It is listed in Table 1 categories 3–7 only.

Which inspection categories apply to St3Gsp?

Table 1 lists St3Gsp in categories 3, 4, 5, 6 and 7 only. Categories 1 and 2 are not listed, so a chemistry-free, impact-free category-1 delivery is not a listed option. Every listed category specifies chemical-composition control and a Table 4 impact test. Category 6 uses Table 3 tensile properties, a different Table 5 bend row, and a thermomechanically treated or heat-treated delivery only. State the category on the order.

What do the plus signs in the St3Gsp Table 2 row mean?

For yield over 40 mm to 100 mm inclusive and over 100 mm, and for elongation over 40 mm, Table 2 marks the cells “+”. Table 2 footnote 2 states that the characteristic is determined for statistical data and that the results are stated in the quality document. Those cells are not specified minima. This page does not replace a plus sign with a number, and a statistical result must not be treated as a design minimum. The specified yield minima are ≥255 N/mm² (≤20 mm) and ≥245 N/mm² (>20–40 mm); elongation minima are ≥23 % (≤20 mm) and ≥24 % (>20–40 mm). Tensile strength is 390–570 N/mm², which is also the agreed range listed for St3Gps and St3Gsp.

Is St3Gsp interchangeable with St3sp or St3Gps?

No. GOST 14637 St3sp Steel Plate is a killed St3 grade without the G, with a lower tensile-strength cell (370–480 N/mm²) and specified yield in every thickness band, and it is listed in categories 1–7. GOST 14637 St3Gps Steel Plate is the manganese semi-killed counterpart (370–490 N/mm², specified yield in every band). Do not fill this grade’s plus-sign cells from those other rows. A manganese (G) mark or a shared St3 class is not interchangeability.

Where is the chemical composition of St3Gsp specified?

Clause 7.1.1.1 requires ladle analysis and product deviations to conform to GOST 380. This page does not tabulate those GOST 380 cells, including the manganese limits for this G designation. Confirm them against the applicable official GOST 380 table. Every listed category already specifies chemistry control. Clause 7.1.1.3 is not written for this grade. Tighter sulphur and phosphorus follow clause 7.1.1.4 when requested for categories 3–5, and at 0.025 % for each element when categories 6 and 7 are ordered. Galvanizing classes B and D are the classes written for killed steel, as an agreed option.

Enquire about GOST 14637 St3Gsp Steel Plate

Enquire for GOST 14637 St3Gsp Steel Plate to GOST 14637-2024. State the category (3–7; categories 1 and 2 are not listed), thickness, width, length or coil mass, quantity, delivery condition and any agreed options. SHH STEEL will review the manganese killed designation, the 390–570 N/mm² Table 2 cell and the statistical (+) bands over 40 mm before quoting production and export.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X