BS 1501 660 Steel Plate
What is BS 1501 660 plate?
We produce and export BS 1501 660 as chromium-molybdenum-vanadium alloy steel plate for pressure purposes. Typical service is alloy pressure equipment that specifies this type.
BS 1501-2:1988 is the last final edition of the alloy-plate part of BS 1501. It was published on 29 July 1988 and superseded on 15 January 1995. It replaced Addendum No. 1 (1973) and Addendum No. 2 (1975) to BS 1501: Part 2: 1970. A photographed 1988 Table 1 was not opened for this page. Clause 3 of the 1988 book is titled Designation, but that clause text was not opened. Clause 19 makes elevated-temperature proof stress an optional requirement for section-two steels. The formal 1988 writing of type, tensile token and any A or B suffix therefore remains unverified. Peer catalogues sometimes write names such as 243 B, 620 B, 621 B or 622-515 B; those B forms are recorded as unverified formal-symbol candidates, not declared absent and not declared commercial-only.
The chemical, room-temperature tensile and elevated-temperature proof figures on this page follow BS EN 10028-2:1993, National Annex NC (normative), opened as a public reprint on 8 November 2026 (Asia/Shanghai). They are a later United Kingdom remaining-steel reference, not a photographed BS 1501-2:1988 Table 1 and not a 1988 guarantee. That annex records steels 271, 281, 621 and 660 as national additional steels after EN 10028-2 superseded part of BS 1501-2. Project acceptance should be agreed against the named edition. These figures are not an SHH proprietary guarantee.
SHH STEEL produces and exports BS 1501 660 plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.
Material specification for BS 1501 660
The items below follow BS 1501-2:1988 as the historical alloy-plate book. Numerical tables in the chemical and mechanical sections follow BS EN 10028-2:1993 National Annex NC as a later United Kingdom remaining-steel reference, not as a photographed 1988 Table 1 and not as a 1988 guarantee. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.
| Parameter | Detail |
|---|---|
| Standard | BS 1501-2:1988, Steels for pressure purposes — Specification for alloy steels: plates. Numerical tables below follow BS EN 10028-2:1993 National Annex NC (normative) as a remaining-steel reference |
| Designation used here | BS 1501 660 |
| Steel type | Chromium-molybdenum-vanadium alloy steel |
| Product form | Alloy steel plate for pressure purposes (this part does not cover bars, sections, forgings, tubes or stainless sheet) |
| How designations are listed | The opened 1993 national annex uses the type number alone (271, 281, 621, 660), without a Part 1-style A or B suffix. Whether the 1988 book used an A or B form for this or other types is unverified. Peer catalogues that print names such as 620 B, 621 B or 622-515 B are recorded as unverified formal-symbol candidates; they are not declared absent and not declared commercial-only |
| Applicable thickness in the opened tensile table | Up to and including 100 mm in the opened tensile table |
| Usual heat treatment | Normalized and tempered at 940–980 °C then 680–720 °C. |
| Chemical analysis | Cast analysis from Table NC.3 of BS EN 10028-2:1993 (remaining-steel reference, not a 1988 guarantee) |
| Tensile properties | Yield strength, tensile strength and elongation from 1993 Table NC.5 |
| Our supply | We produce and export 660 plate to the ordered edition, delivery condition, dimensions and extra tests |
Chemical composition of BS 1501 660
The chemical, room-temperature tensile and elevated-temperature proof figures on this page follow BS EN 10028-2:1993, National Annex NC (normative), opened as a public reprint on 8 November 2026 (Asia/Shanghai). They are a later United Kingdom remaining-steel reference, not a photographed BS 1501-2:1988 Table 1 and not a 1988 guarantee. That annex records steels 271, 281, 621 and 660 as national additional steels after EN 10028-2 superseded part of BS 1501-2. Project acceptance should be agreed against the named edition. These figures are not an SHH proprietary guarantee. Where a maximum aluminium (metal) content of 0.020 % is specified, determination of total aluminium, provided it does not exceed that value, shall be deemed to meet the requirement; in dispute, metallic aluminium shall be determined. A public-database listing showed C 0.10–0.15, Cr 0.30–0.50, Cu ≤ 0.30 and Rm 460–660 MPa, which conflicts with Tables NC.3 and NC.5 and is not used here.
| Element | Value (wt. %) | Source opened for this cell |
|---|---|---|
| Carbon (C) | 0.08–0.13 | BS EN 10028-2:1993 Table NC.3 |
| Silicon (Si) | 0.30 max | BS EN 10028-2:1993 Table NC.3 |
| Manganese (Mn) | 0.60–1.00 | BS EN 10028-2:1993 Table NC.3 |
| Phosphorus (P) | 0.025 max | BS EN 10028-2:1993 Table NC.3 |
| Sulfur (S) | 0.015 max | BS EN 10028-2:1993 Table NC.3 |
| Chromium (Cr) | 0.25–0.50 | BS EN 10028-2:1993 Table NC.3 |
| Molybdenum (Mo) | 0.50–0.70 | BS EN 10028-2:1993 Table NC.3 |
| Nickel (Ni) | 0.30 max | BS EN 10028-2:1993 Table NC.3 |
| Copper (Cu) | 0.20 max | BS EN 10028-2:1993 Table NC.3 |
| Aluminium (metal) (Al) | 0.020 max | BS EN 10028-2:1993 Table NC.3 |
| Vanadium (V) | 0.22–0.28 | BS EN 10028-2:1993 Table NC.3 |
Tensile, impact and elevated-temperature properties for BS 1501 660
Room-temperature tensile properties below are from Table NC.5 of BS EN 10028-2:1993. Strength values are in N/mm², equivalent to MPa. No further thickness row was opened.
| Thickness | Tensile strength Rm, N/mm² | Yield strength Re, N/mm² min | Elongation A, % min | Source |
|---|---|---|---|---|
| Up to and including 100 mm | 460–610 | 310 | 19 | BS EN 10028-2:1993 Table NC.5 |
Table NC.6 has no 660 impact row; that cell is omitted rather than invented. Minimum Re or Rp0.2 at elevated temperature from Table NC.8, for thickness up to and including 100 mm, is 282, 276, 267, 241, 225, 216, 209, 203, 200 and 197 N/mm² at 100, 150, 200, 250, 300, 350, 400, 450, 500 and 550 °C. Those figures are from the 1993 national annex, not from BS 1501-1 appendices. Informative stress-rupture values in Table NC.11 are noted but not copied. The chemical, room-temperature tensile and elevated-temperature proof figures on this page follow BS EN 10028-2:1993, National Annex NC (normative), opened as a public reprint on 8 November 2026 (Asia/Shanghai). They are a later United Kingdom remaining-steel reference, not a photographed BS 1501-2:1988 Table 1 and not a 1988 guarantee. That annex records steels 271, 281, 621 and 660 as national additional steels after EN 10028-2 superseded part of BS 1501-2. Project acceptance should be agreed against the named edition. These figures are not an SHH proprietary guarantee.
Delivery conditions for BS 1501 660
Steels 271, 281, 621 and 660 shall be supplied normalized and tempered in accordance with Table NC.1. For type 660 the opened ranges are normalizing at 940–980 °C and tempering at 680–720 °C. Name the required delivery condition on the purchase order.
If the project has moved to EN 10028-2, order the successor designation and edition expressly. A later European name is not by itself a substitute instruction for type 660.
The purchase order should name the official designation, the edition required, thickness, width and length, the delivery condition, any extra tests, and the inspection document required.
This page does not offer heat-treatment or fabrication services.
Welding and thermal cutting
Neither the opened historical book notes nor the later remaining-steel annex set a welding procedure for type 660 on this page. Welding and thermal cutting should be qualified for the alloy content, thickness and the specified delivery condition.
Type 660 is a vanadium-bearing chromium-molybdenum plate. Consumables and hydrogen control should match the qualified procedure for that alloy family.
Heat input and any required post-weld heat treatment belong in the project specification.
Form, appearance, dimensions and thickness tolerances
Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate tolerances when that standard is specified.
Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.
Applications and specification limits
We produce and export 660 plate as alloy steel plate for pressure purposes. Typical service is alloy pressure equipment that specifies type 660.
BS 1501-2:1988 is a historical alloy-plate standard. It is not the current EN 10028-2 or EN 10028-4 order unless that successor standard is written on the enquiry, and it is not a BS 1501-1 carbon, BS 1501-3 stainless, BS 1502 bar or BS 1503 forging order.
Compare BS 1501 660 with other steel plates
BS 1501 660 is a historical BS 1501-2 alloy pressure-vessel plate. The comparison below is for selection only; these materials are not equivalents.
| Material | Alloy / type | Delivery condition | Mechanical requirements | Typical service | Substitution limit |
|---|---|---|---|---|---|
| BS 1501 660 (this plate) | Cr-Mo-V alloy plate | Normalized and tempered at 940–980 °C then 680–720 °C. | Up to 100 mm: yield 310 N/mm² minimum; tensile 460–610 N/mm² (1993 Table NC.5) | Alloy pressure equipment that specifies this type | A later EN name or a different 1988 type is not an automatic substitute |
| EN 10028-2 16Mo3 | Molybdenum elevated-temperature vessel plate, steel number 1.5415 | As specified in EN 10028-2 | Live published yield 275 MPa at ≤ 16 mm and tensile 440–590 MPa | Modern European molybdenum vessel plate | Different alloy; 16Mo3 numbers are not copied onto type 660 |
| EN 10028-2 13CrMo4-5 | Chromium-molybdenum elevated-temperature vessel plate, steel number 1.7335 | As specified in EN 10028-2 | Live published yield 300 MPa at ≤ 16 mm and tensile 450–600 MPa | Modern European 1Cr-0.5Mo vessel plate | Related chromium-molybdenum class only |
| EN 10028-2 10CrMo9-10 | 2.25Cr-1Mo elevated-temperature vessel plate, steel number 1.7380 | As specified in EN 10028-2 | Live published yield 310 MPa at ≤ 16 mm and tensile 480–630 MPa | Modern European 2.25Cr-1Mo vessel plate | Higher chromium than type 660; not an automatic substitute |
Equivalent and related grades by country
The designations below are near names, not automatic substitutes. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form. The 1993 annex lists 660 without an A or B suffix.
| Country / region | Standard | Grade or designation | Similarity and key differences | Substitution caveat |
|---|---|---|---|---|
| United Kingdom | BS 1501-2:1988 / BS EN 10028-2:1993 National Annex NC | 660 | This plate, from the 1993 remaining-steel annex. Cr-Mo-V with tensile 460–610 N/mm² up to 100 mm. | This product |
| Europe | EN 10028-2 | 16Mo3 (1.5415) | Later molybdenum vessel plate. Live published yield 275 MPa at ≤ 16 mm and tensile 440–590 MPa. | Near name only; not an automatic substitute |
| Europe | EN 10028-2 | 13CrMo4-5 (1.7335) | Later 1Cr-0.5Mo vessel plate. Live published yield 300 MPa at ≤ 16 mm and tensile 450–600 MPa. | Related chromium-molybdenum class only |
| United States / China | — | — | No separately verified ASTM or GB plate counterpart was established as an automatic equivalent for type 660 on this page. | Do not assume a local chrome-moly or vanadium-molybdenum name is a substitute |
Why choose SHH STEEL for BS 1501 660
- We produce and export BS 1501 660 alloy pressure-vessel steel plate
- We review the enquiry for edition, designation, delivery condition, dimensions and extra tests
- We keep the historical BS 1501-2 type number distinct from later EN 10028-2 names and from Part 1 A/B carbon grades, and we record peer B forms as unverified formal-symbol candidates until a 1988 table is opened
- We match documentation to what the purchase order requires
How to enquire for BS 1501 660 plate
| Item | What to specify |
|---|---|
| Standard and designation | BS 1501 660 and the edition required (BS 1501-2:1988 and/or the 1993 national-annex remaining-steel clauses) |
| Or successor standard | The EN 10028-2 designation and edition, if that is what the project now requires |
| Delivery condition | Normalized and tempered at 940–980 °C then 680–720 °C. |
| Dimensions | Required thickness, width and length |
| Chemistry | Cast analysis to the named edition |
| Mechanical tests | Yield strength, tensile strength, elongation and, where specified, impact or elevated-temperature proof tests to the named edition |
| Other tests | Ultrasonic examination or other extra tests only when written on the order |
| Documentation | State the inspection document type required by the project |
Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.
Frequently Asked Questions
-
Is BS 1501-2 still a current product standard?
- No. BS 1501-2:1988 is the last final edition of the alloy-plate part. It was published on 29 July 1988 and superseded on 15 January 1995. EN 10028-2 superseded part of it. Projects still using a historical type number should name the edition required on the order.
-
Which edition do the tables on this page follow?
- They follow BS EN 10028-2:1993 National Annex NC (Tables NC.1, NC.3, NC.5 and NC.8), opened as a public reprint. That is a later remaining-steel reference, not a photographed 1988 Table 1 and not a 1988 guarantee. Specify the edition required on the purchase order.
-
Is type 660 the same as 660A, 660B or 14MoV6-3?
- The opened 1993 annex lists the steel as 660, without an A or B suffix. Whether the 1988 book used a B form is unverified. 14MoV6-3 is a related chemistry-family name in other books, not an automatic substitute.
-
Does this page copy Part 1 elevated-temperature appendix figures?
- No. Elevated proof-stress values come from Table NC.8 of the 1993 national annex for type 660. Informative stress-rupture values in Table NC.11 are noted but not copied.
-
What should a quotation enquiry include?
- BS 1501 660, the edition required or the successor designation, the delivery condition, plate thickness by width by length, quantity, any extra tests, and the inspection document required.
Request a quotation
Contact SHH STEEL for a quotation for BS 1501 660 steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.
Specify the edition (BS 1501-2:1988 or the later United Kingdom national-annex remaining-steel clauses, or a named EN 10028-2 successor if that is what the project now requires), the delivery condition and any specimen heat treatment. If your project requires ultrasonic examination, a stated impact temperature or another extra test, include the acceptance criteria and the inspection document required.
If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.