ASTM A265 SA516 Gr.70 + Nickel 200 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.70 + Nickel 200 clad plate bonds commercially pure nickel (UNS N02200) to a carbon steel pressure vessel base. Pure nickel is the classic material for caustic soda evaporators and concentrators below about 315 °C. SHH STEEL produces it by explosion bonding, with 140 MPa shear and ultrasonic tests when ordered.
Keywords
Nickel 200 clad plate, pure nickel clad steel plate, ASTM A265 Nickel 200, SA516 Gr.70 + N02200, nickel clad plate for caustic
Equivalent Grades:
ASME SA-265, JIS G3602, NB/T 47002.2; Nickel 200 = N02200 / 2.4066 / N6
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A265 SA516 Gr.70 + Nickel 200 nickel alloy clad plate?

ASTM A265 SA516 Gr.70 + Nickel 200 nickel alloy clad plate is a composite plate in which Nickel 200 (UNS N02200), commercially pure wrought nickel, is metallurgically bonded to an SA516 Grade 70 carbon steel base. The carbon steel carries pressure and structural loads; the nickel alloy face resists the corrosive medium. It is ordered to ASTM A265, or the identical ASME SA-265, the specification for nickel and nickel-base alloy-clad steel plate.

On drawings it appears as SA516 Gr.70 + N02200 or SA516 Gr.70 + Ni200, with the thickness pair such as 3 + 20 mm. Nickel 200 is at least 99 % nickel. Its value lies in one environment above all: caustic soda. Pure nickel corrodes at extremely low rates in sodium and potassium hydroxide across most concentrations, and it does not suffer the caustic stress corrosion cracking that attacks carbon and stainless steels.

In a caustic evaporator, a nickel clad shell gives that resistance at a fraction of the price of solid nickel, and the steel back carries the pressure. Nickel also keeps caustic product free of iron contamination, which matters for rayon, soap and food-grade alkali.

SHH STEEL can produce Nickel 200 clad plate by explosion bonding, the usual route for nickel alloy claddings, and certifies each plate to the A265 tests on the order. Other nickel alloy claddings are listed under nickel alloy clad plates.

ASTM A265 / ASME SA-265 requirements for Nickel 200 clad plate

ASTM A265 covers plate of a carbon or low-alloy steel base with nickel or a nickel-base alloy integrally and continuously bonded to one or both faces. It is written mainly for pressure vessels but may be used in other structural applications where corrosion resistance is needed. ASME publishes it as SA-265, identical with ASTM A265-12(2019).

Item Requirement for SA516 Gr.70 + Nickel 200
Cladding B162 / SB-162 UNS N02200 (Nickel 200)
Other permitted claddings Alloys of B127, B162, B168, B333, B409, B424, B443, B463, B575, B582, B625, or others agreed
Base steel SA516 Grade 70; the standard allows pressure vessel or general structural steels (A20/A20M or A6/A6M)
Product size “Plate” means 3/16 in (4.8 mm) and over in thickness and over 10 in (254 mm) wide
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser requires them
Bond integrity Visual below 10 mm total; ultrasonic to A578/A578M procedures at 10 mm and over; Class 1, 3 or 5
Clad surface As-rolled, blasted (descaled and pickled) or 100 % conditioned, unless otherwise specified
Marking Per A20 or A6 for the base, plus the alloy designation and the specification number

A complete order line reads: “Clad plate to ASME SA-265, cladding SB-162 UNS N02200, annealed, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1 bond quality, 100 % UT (S12); shear test required.” State the design temperature: above about 315 °C the cladding should be Nickel 201.

SA516 Gr.70 base and Nickel 200 cladding

A265 certifies each layer to its own specification: the cladding to ASTM B162 and the base to ASTM A516 / ASME SA-516. The pairing puts an expensive corrosion alloy only on the wetted face.

Why Nickel 200 is chosen

Nickel 200 contains at least 99.0 % nickel, with copper up to 0.25 %, iron up to 0.40 %, manganese up to 0.35 %, silicon up to 0.35 % and carbon up to 0.15 %. In the annealed condition it is soft and ductile, with good thermal and electrical conductivity.

Its weakness is temperature. With up to 0.15 % carbon, Nickel 200 held for long periods above about 315 °C (600 °F) can precipitate graphite at grain boundaries and become brittle. ASME therefore limits Nickel 200 to that temperature range, and the low-carbon Nickel 201 is used above it. Nickel is also attacked by oxidizing acids, by ammonia-bearing solutions and by sulfur-bearing gases at high temperature.

SA516 Grade 70 base steel

ASME SA516 Grade 70 is the usual base: a carbon-manganese vessel plate with 485 to 620 MPa tensile and 260 MPa minimum yield, available normalized and impact tested. Outside ASME work it is bought as ASTM A516 Grade 70. For high-temperature hydrogen or creep service, a Cr-Mo base such as ASTM A387 Grade 11 Class 2 can replace it.

Nickel 200 compared with other nickel claddings

Cladding Key alloying, % Typical reason to choose it
Nickel 200 (N02200) Ni 99.0 min, C 0.15 max Caustic soda below about 315 °C
Nickel 201 (N02201) Ni 99.0 min, C 0.02 max Caustic service above about 315 °C
Alloy 600 (N06600) Ni 72 min, Cr 14–17 Caustic with oxidizing species, high temperature
Alloy 400 (N04400) Ni 63 min, Cu 28–34 Hydrofluoric acid, seawater

How Nickel 200 clad plate is made

Explosion bonding is the main manufacturing route for nickel alloy clad plate, because it joins alloys of very different strength and melting behaviour without melting either one. Roll bonding is also possible for some nickel alloys and plate sizes, and weld overlay is the alternative for shapes that cannot be clad as plate.

Explosion bonding

The Nickel 200 sheet is positioned above the SA516 plate with a controlled gap and covered with explosive. The detonation accelerates the cladding onto the base at an oblique angle; surface oxides are jetted away and the metals bond in the solid state with a wavy interface. There is no dilution, so the cladding chemistry at the surface is exactly that of the sheet. A265 permits the cladding to be made from several sheets welded together for plates wider than the available alloy sheet, with that welding qualified to ASME Section IX.

Clad plate or weld overlay?

Nickel weld overlay with ERNi-1 is possible, but iron from the steel dilutes the first layers, and caustic service needs a low-iron surface. Clad plate gives full-purity nickel across the whole shell, inspected by ultrasonic testing before fabrication.

Chemical composition of Nickel 200 cladding and SA516 Gr.70 base

The chemical composition is certified layer by layer by the clad plate manufacturer: the cladding to ASTM B162 and the base to SA-516.

Nickel 200 cladding (UNS N02200), heat analysis

Element Nickel 200 (UNS N02200), % (ASTM B162)
Nickel (Ni), incl. cobalt 99.0 min
Copper (Cu) 0.25 max
Iron (Fe) 0.40 max
Manganese (Mn) 0.35 max
Carbon (C) 0.15 max
Silicon (Si) 0.35 max
Sulfur (S) 0.01 max

These are the B162 limits for UNS N02200. Product analysis, when required, is made to ASTM B880 tolerances.

Product analysis of the cladding is made only when the purchaser asks for it, and the results must meet the cladding specification. For wet chemical analysis A265 asks the laboratory to discard all base metal plus 40 % of the cladding thickness from the bonded side, up to 1.6 mm, so that iron from the steel does not distort the result; spectrometric samples are taken on the centre line of the cladding.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength

A265 tests the tensile properties, the bond strength and the bond integrity of the plate in its delivered condition.

Tensile test

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base minimum up to base maximum plus 35 MPa
Composite over 38 mm, or stronger base Base steel only All base steel tensile requirements
Cladding for corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property Nickel 200 cladding (ASTM B162) SA516 Gr.70 base
Tensile strength 380 MPa (55 ksi) min (hot-rolled, annealed plate) 485 – 620 MPa
Yield strength (0.2 % offset) 100 MPa (15 ksi) min 260 MPa min
Elongation 40 % min 21 % min in 50 mm; 17 % min in 200 mm
Hardness Not specified for acceptance in B162 Not specified

Nickel 200 is much softer than SA516 Gr.70. For a composite tensile test, the A265 rule applies: the result must lie between the minimum and maximum calculated from both layers. Because the cladding is weak, its contribution lowers the composite minimum slightly; this is normal and is allowed for in the rule.

Shear and bend tests

When required, the minimum shear strength between cladding and base is 20 000 psi (140 MPa), with at least 1.9 mm of cladding on the specimen and one test per plate as rolled. As an alternative, three bond bend tests through 180° with the cladding in compression are made; at least two must show no more than 50 % separation on either edge.

Ultrasonic bond quality

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

The class must be listed on the order; when none is given, plates may be supplied as Class 5. Scanning extent is the manufacturer’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. Caustic evaporators are normally ordered Class 1 with 100 % coverage, since any unbonded area under a hot caustic film is a potential crack starter.

Heat treatment of Nickel 200 clad plate

A265 does not impose a single heat treatment. Unless the cladding or base specification requires a specific treatment, or the purchaser and manufacturer agree otherwise, the clad plate is furnished in a condition appropriate for the cladding alloy, the base metal, or both.

Nickel 200 clad plate is supplied as-clad and flattened, or stress relieved by agreement, with the nickel sheet annealed before bonding. Nickel tolerates the SA516 stress relief and PWHT temperatures.

Keep all sulfur-bearing contamination, such as marking crayons, oils, grease and some furnace atmospheres, away from the nickel before any heat treatment. Sulfur embrittles nickel at high temperature.

If the vessel will be post-weld heat treated, order Supplementary Requirement S3 so the test coupons see a simulated PWHT, and state temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Cladding, base and total thickness may each be ordered as minimum or nominal values.

Item ASTM A265 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness A20/A20M or A6/A6M, as appropriate for the base

Order the Nickel 200 cladding as a minimum thickness, typically 2 to 3 mm for evaporator shells. The nickel surface is supplied as-rolled, blasted or conditioned as agreed.

Stock sizes and thickness combinations of Nickel 200 clad plate

SA516 Gr.70 + Nickel 200 clad plate is ordered by cladding plus base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 10 12 Caustic tanks
2 + 12 14 Evaporator bodies
3 + 14 17 Vessel shells
3 + 16 19 Concentrators
3 + 20 23 Pressure vessels
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Tube sheets
6 + 50 56 Tube sheets
8 + 70 and over 78 and over Heavy sections, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

For nickel alloys, the cladding is usually 2 to 6 mm because of alloy cost; tube sheets take thicker layers so that tube-to-tubesheet welds stay inside the alloy.

Welding SA516 Gr.70 + Nickel 200 clad plate

Clad joints are welded in two parts: a carbon steel weld for strength, then a nickel alloy overlay that restores the Nickel 200 face. Carbon steel filler must not reach the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back from the root.
  2. Weld the SA516 Gr.70 with matching carbon steel filler.
  3. Back-gouge the clad side to sound weld metal.
  4. Overlay the carbon steel weld with ERNi-1 (AWS A5.14) or ENi-1 (AWS A5.11), which match commercially pure nickel, using enough layers to bring iron dilution at the surface within the limit the service needs.
  5. Clean the finished overlay; nickel alloys are not normally pickled like stainless steel, but heat tint and slag must be removed.

ERNi-1 contains titanium to control porosity and tolerates moderate iron dilution, but two layers are usually needed over the steel weld for a caustic-resistant surface. Nickel weld metal is sluggish; use wide bevel angles and clean, bright surfaces.

Procedures and welders are qualified to ASME Section IX, which A265 also requires for welded cladding and for cladding repairs. Repairs are checked by liquid penetrant and reported on the certificate.

Applications of Nickel 200 clad plate

Nickel 200 clad plate is used where caustic resistance or product purity is needed in thick or large vessels.

  • Caustic soda evaporators and concentrators in chlor-alkali plants.
  • Caustic storage and transport tanks for high-purity product.
  • Synthetic fiber and rayon processing vessels.
  • Soap and detergent plants handling hot alkali.
  • Food processing where alkali must stay iron-free.
  • Alumina refining equipment exposed to caustic liquors.

Nickel 200 or Nickel 201?

Both resist caustic equally. Below about 315 °C either works and Nickel 200 is more widely stocked; above it, Nickel 201’s 0.02 % carbon limit prevents graphitization. When in doubt about upset temperatures, specify Nickel 201.

Testing and certification

The A265 certificate reports the chemical analysis of both layers, the Section 7 test results, the bond quality class and any additional tests on the order.

Test or document Basis Frequency / note
Chemical analysis of both layers SA-516 and ASTM B162 Each heat; product analysis (S2) if ordered
Tensile test A265 and the base specification Each plate as rolled
Shear test or three bond bend tests A265 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Iron at the cladding surface Agreed method When ordered
Penetrant test of cladding repairs A265 Section 14 Each repair, reported with location and procedure
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

If your project does not accept weld repairs of the cladding, or wants to approve them first, state that restriction on the order; A265 lists it as a purchaser option.

Equivalent standards and grades

Other standards describe the same product with their own test levels; use them to cross-check, not to substitute without review.

Standard Scope Bond shear requirement
ASTM A265 / ASME SA-265 Nickel and nickel-base alloy-clad steel plate 140 MPa min, when specified
JIS G3602 Nickel and nickel alloy clad steels Per JIS G3602
NB/T 47002.2 Clad plate for pressure equipment, nickel-steel Per NB/T 47002.2
Layer ASTM / ASME UNS EN / W.Nr. JIS GB
Cladding B162 / SB-162 UNS N02200 (Nickel 200) UNS N02200 2.4066 (Ni 99.2) NW2200 N6
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Chinese projects order the same product under NB/T 47002.2 with N6 cladding; Japanese projects use JIS G3602 with NW2200. Stainless claddings for milder duty are covered under ASTM A264.

Why order Nickel 200 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying nickel alloy clad plate to vessel, heat exchanger and FGD fabricators. For Nickel 200 orders we confirm the design temperature first, and recommend Nickel 201 where it is needed.

  • We check the enquiry against ASTM A265 and flag missing items: cladding specification, bond class, shear test, PWHT simulation.
  • We quote cladding and base thicknesses separately, as minimum or nominal.
  • The nickel alloy sheet and the base plate come with traceable mill certificates; UT maps are supplied when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut to drawing.

FAQ

Why is Nickel 200 used for caustic soda?
Pure nickel corrodes very slowly in sodium and potassium hydroxide over most concentrations and temperatures, and it does not suffer caustic stress corrosion cracking.
What is the temperature limit of Nickel 200?
About 315 °C (600 °F). Above that, its carbon can precipitate as graphite at grain boundaries; Nickel 201 is used instead.
Which filler is used for Nickel 200 clad plate?
ERNi-1 or ENi-1 over the steel weld, in two or more layers for a low-iron surface.
What are the mechanical properties of Nickel 200 plate?
B162 hot-rolled annealed plate: 380 MPa minimum tensile, 100 MPa minimum yield and 40 % elongation.
Is ASME SA-265 the same as ASTM A265?
Yes in content. ASME publishes A265 as SA-265 in Section II Part A, identical with ASTM A265-12(2019). Order SA-265 for ASME Code vessels.
What is the HS code for nickel alloy clad plate?
Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
ASTM A265 or ASME SA-265, Nickel 200 cladding thickness and specification, base grade and thickness, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, and certificate type.

Request a quotation for ASTM A265 SA516 Gr.70 + Nickel 200 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.70 + Nickel 200 nickel alloy clad plate bonds B162 commercially pure nickel to an SA516 Grade 70 base, with 140 MPa shear when specified and ultrasonic Class 1, 3 or 5. It is the economical caustic-resistant plate for evaporators and vessels below about 315 °C.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other claddings on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X