ASTM A265 SA516 Gr.70 + Alloy 59 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.70 + Alloy 59 clad plate bonds low-carbon nickel-chromium-molybdenum alloy 59 (UNS N06059) to a carbon steel pressure vessel base. With 23 % chromium and 16 % molybdenum it resists oxidizing and reducing acids and severe chlorides. SHH STEEL produces it by explosion bonding with shear and UT tests as ordered.
Keywords
Alloy 59 clad plate, alloy 59 clad steel plate, ASTM A265 alloy 59, SA516 Gr.70 + N06059, Ni-Cr-Mo clad plate
Equivalent Grades:
ASME SA-265, JIS G3602, NB/T 47002.2 (by agreement); alloy 59 = N06059 / 2.4605
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A265 SA516 Gr.70 + Alloy 59 nickel alloy clad plate?

ASTM A265 SA516 Gr.70 + Alloy 59 nickel alloy clad plate is a composite plate in which alloy 59 (UNS N06059), a low-carbon nickel-chromium-molybdenum alloy, is metallurgically bonded to an SA516 Grade 70 carbon steel base. The carbon steel carries the pressure; the alloy 59 face resists the corrosive medium. It is ordered to ASTM A265 or the identical ASME SA-265.

It is written SA516 Gr.70 + N06059 or SA516 Gr.70 + alloy 59 with the thickness pair. Alloy 59 sits in the same family as C-276 and C-22, but with about 23 % chromium and 16 % molybdenum and almost no iron or tungsten. That balance gives it strong resistance to both oxidizing and reducing media and one of the highest pitting resistance values of the Ni-Cr-Mo alloys.

The very low iron and the absence of tungsten also make it thermally stable: it forms intermetallic phases more slowly than C-276 when heated, which is useful for clad plate that sees bonding, flattening, welding and sometimes PWHT.

SHH STEEL can produce alloy 59 clad plate by explosion bonding and certifies each plate to the A265 tests on the order. Other claddings are listed under nickel alloy clad plates.

ASTM A265 / ASME SA-265 requirements for Alloy 59 clad plate

ASTM A265 covers plate of a carbon or low-alloy steel base with nickel or a nickel-base alloy integrally and continuously bonded to one or both faces. It is written mainly for pressure vessels but may be used in other structural applications where corrosion resistance is needed. ASME publishes it as SA-265, identical with ASTM A265-12(2019).

Item Requirement for SA516 Gr.70 + Alloy 59
Cladding B575 / SB-575 UNS N06059 (alloy 59)
Other permitted claddings Alloys of B127, B162, B168, B333, B409, B424, B443, B463, B575, B582, B625, or others agreed
Base steel SA516 Grade 70; the standard allows pressure vessel or general structural steels (A20/A20M or A6/A6M)
Product size “Plate” means 3/16 in (4.8 mm) and over in thickness and over 10 in (254 mm) wide
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser requires them
Bond integrity Visual below 10 mm total; ultrasonic to A578/A578M procedures at 10 mm and over; Class 1, 3 or 5
Clad surface As-rolled, blasted (descaled and pickled) or 100 % conditioned, unless otherwise specified
Marking Per A20 or A6 for the base, plus the alloy designation and the specification number

A complete order line reads: “Clad plate to ASME SA-265, cladding SB-575 UNS N06059, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1 bond quality, 100 % UT (S12); shear test required; simulated PWHT per S3.” State whether the cladding counts toward design strength or is corrosion allowance only.

SA516 Gr.70 base and Alloy 59 cladding

A265 certifies each layer to its own specification: the cladding to ASTM B575 and the base to ASTM A516 / ASME SA-516. The pairing puts an expensive corrosion alloy only on the wetted face.

Why Alloy 59 is chosen

Alloy 59 contains 22.0 to 24.0 % chromium and 15.0 to 16.5 % molybdenum, with nickel as the balance, iron up to 1.5 % and a small aluminum addition. Carbon is limited to 0.010 % and silicon to 0.10 %.

High chromium resists oxidizing acids and chlorine dioxide; high molybdenum resists reducing acids and chloride pitting and crevice corrosion. Low iron keeps the matrix stable, so the heat-affected zones of welds keep their resistance without a post-weld anneal.

Owners choose alloy 59 for mixed or variable process streams, where the medium may swing between oxidizing and reducing conditions, and for FGD and waste incineration zones where C-276 is at its limit.

SA516 Grade 70 base steel

ASME SA516 Grade 70 is the usual base: a carbon-manganese vessel plate with 485 to 620 MPa tensile and 260 MPa minimum yield, available normalized and impact tested. Outside ASME work it is bought as ASTM A516 Grade 70. For high-temperature hydrogen or creep service, a Cr-Mo base such as ASTM A387 Grade 11 Class 2 can replace it.

Alloy 59 compared with other Ni-Cr-Mo claddings

Cladding Mo, % Cr, % Best fit
Alloy 59 (N06059) 15.0 – 16.5 22.0 – 24.0 Mixed oxidizing and reducing media, severe pitting
Alloy C-276 (N10276) 15.0 – 17.0 14.5 – 16.5 Reducing acids, wet chlorine, FGD
Alloy C-22 (N06022) 12.5 – 14.5 20.0 – 22.5 Oxidizing chlorides, mixed acids
Alloy 625 (N06625) 8.0 – 10.0 20.0 – 23.0 Seawater and chloride pitting

Design notes for alloy 59 clad plate

Alloy 59 is usually specified as corrosion allowance, 2 to 3 mm thick. For FGD and incineration scrubbers it is often used in the worst zones, with less expensive claddings elsewhere on the same carbon steel structure.

Because its corrosion resistance is close to the top of the Ni-Cr-Mo family, it is also used as a single cladding for multipurpose vessels where the product slate changes, avoiding the risk of choosing a narrower alloy.

How Alloy 59 clad plate is made

Explosion bonding is the main manufacturing route for nickel alloy clad plate, because it joins alloys of very different strength and melting behaviour without melting either one. Roll bonding is also possible for some nickel alloys and plate sizes, and weld overlay is the alternative for shapes that cannot be clad as plate.

Explosion bonding

The Alloy 59 sheet is positioned above the SA516 plate with a controlled gap and covered with explosive. The detonation accelerates the cladding onto the base at an oblique angle; surface oxides are jetted away and the metals bond in the solid state with a wavy interface. There is no dilution, so the cladding chemistry at the surface is exactly that of the sheet. A265 permits the cladding to be made from several sheets welded together for plates wider than the available alloy sheet, with that welding qualified to ASME Section IX.

Clad plate or weld overlay?

Alloy 59 weld overlay is used on nozzles and flange faces, but dilution from the steel reduces its resistance and several layers are needed. An explosion bonded alloy 59 clad plate gives full-chemistry alloy across the whole surface without that loss.

Chemical composition of Alloy 59 cladding and SA516 Gr.70 base

The chemical composition is certified layer by layer by the clad plate manufacturer: the cladding to ASTM B575 and the base to SA-516.

Alloy 59 cladding (UNS N06059), heat analysis

Element Alloy 59 (UNS N06059), % (ASTM B575)
Nickel (Ni) Balance
Chromium (Cr) 22.0 – 24.0
Molybdenum (Mo) 15.0 – 16.5
Iron (Fe) 1.5 max
Aluminum (Al) 0.1 – 0.4
Cobalt (Co) 0.3 max
Manganese (Mn) 0.5 max
Copper (Cu) 0.50 max
Carbon (C) 0.010 max
Silicon (Si) 0.10 max
Phosphorus (P) 0.015 max
Sulfur (S) 0.010 max

The limits are those of ASTM B575 for UNS N06059; confirm the current edition before quoting single elements. Low iron, carbon and silicon are what give alloy 59 its stability, so check them on the sheet certificate.

Product analysis of the cladding is made only when the purchaser asks for it, and the results must meet the cladding specification. For wet chemical analysis A265 asks the laboratory to discard all base metal plus 40 % of the cladding thickness from the bonded side, up to 1.6 mm, so that iron from the steel does not distort the result; spectrometric samples are taken on the centre line of the cladding.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength

A265 tests the tensile properties, the bond strength and the bond integrity of the plate in its delivered condition.

Tensile test

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base minimum up to base maximum plus 35 MPa
Composite over 38 mm, or stronger base Base steel only All base steel tensile requirements
Cladding for corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property Alloy 59 cladding (ASTM B575) SA516 Gr.70 base
Tensile strength 690 MPa min 485 – 620 MPa
Yield strength (0.2 % offset) 310 MPa min 260 MPa min
Elongation 45 % min 21 % min in 50 mm; 17 % min in 200 mm
Hardness Not specified for clad plate Not specified

A 3 + 20 mm plate is tested full thickness, with the composite between 485 and 655 MPa. Alloy 59 is stronger than SA516 Gr.70, so thick claddings raise the composite; the corrosion-allowance-only option of A265 is worth considering for tube sheets.

Shear and bend tests

When required, the minimum shear strength between cladding and base is 20 000 psi (140 MPa), with at least 1.9 mm of cladding on the specimen and one test per plate as rolled. As an alternative, three bond bend tests through 180° with the cladding in compression are made; at least two must show no more than 50 % separation on either edge.

Ultrasonic bond quality

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

The class must be listed on the order; when none is given, plates may be supplied as Class 5. Scanning extent is the manufacturer’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. FGD and chemical plates with alloy 59 cladding are normally ordered Class 1 with 100 % coverage.

Heat treatment of Alloy 59 clad plate

A265 does not impose a single heat treatment. Unless the cladding or base specification requires a specific treatment, or the purchaser and manufacturer agree otherwise, the clad plate is furnished in a condition appropriate for the cladding alloy, the base metal, or both.

SA516 Gr.70 + alloy 59 plate is usually delivered as-clad and flattened, with the alloy sheet solution annealed before bonding. A solution anneal of the clad plate after bonding is not practical because of its effect on the steel.

Alloy 59 is more tolerant of intermediate-temperature exposure than C-276, but long PWHT can still precipitate secondary phases. For vessels that need PWHT, simulate the cycle on S3 coupons and consider a corrosion test of the cladding afterwards.

If the vessel will be post-weld heat treated, order Supplementary Requirement S3 so the test coupons see a simulated PWHT, and state temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Cladding, base and total thickness may each be ordered as minimum or nominal values.

Item ASTM A265 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness A20/A20M or A6/A6M, as appropriate for the base

Order the alloy 59 cladding to a minimum thickness, typically 2 mm for FGD ducts and 3 mm for pressure vessels. Tube sheet faces can be machined; add the allowance to the minimum.

Stock sizes and thickness combinations of Alloy 59 clad plate

SA516 Gr.70 + Alloy 59 clad plate is ordered by cladding plus base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 8 10 Scrubber ducts
2 + 10 12 FGD absorber zones
2 + 14 16 Incinerator quench vessels
3 + 16 19 Chemical reactors
3 + 20 23 Pressure vessels
4 + 30 34 Heads
5 + 40 45 Tube sheets
6 + 60 66 Heavy tube sheets
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

For nickel alloys, the cladding is usually 2 to 6 mm because of alloy cost; tube sheets take thicker layers so that tube-to-tubesheet welds stay inside the alloy.

Welding SA516 Gr.70 + Alloy 59 clad plate

Clad joints are welded in two parts: a carbon steel weld for strength, then a nickel alloy overlay that restores the Alloy 59 face. Carbon steel filler must not reach the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back from the root.
  2. Weld the SA516 Gr.70 with matching carbon steel filler.
  3. Back-gouge the clad side to sound weld metal.
  4. Overlay the carbon steel weld with ERNiCrMo-13 (AWS A5.14) or ENiCrMo-13 (AWS A5.11), matching alloy 59, in two or more layers to keep surface iron low.
  5. Clean the finished overlay; nickel alloys are not normally pickled like stainless steel, but heat tint and slag must be removed.

Low heat input and stringer beads limit segregation in the weld. Alloy 59 filler is also used to weld C-276 and C-22 claddings, because its weld metal resists corrosion at least as well as those base alloys.

Batten strips of alloy 59 sheet over clad seams are an alternative in FGD ducts, agreed in the fabrication design.

Procedures and welders are qualified to ASME Section IX, which A265 also requires for welded cladding and for cladding repairs. Repairs are checked by liquid penetrant and reported on the certificate.

Applications of Alloy 59 clad plate

Alloy 59 clad plate is used where the process medium is severe, mixed or variable, and a single cladding must cover all cases.

  • Flue gas desulfurization inlet zones, ducts and stacks.
  • Waste incineration scrubbers and quench vessels.
  • Chemical reactors with mixed oxidizing and reducing acids.
  • Pulp bleaching with chlorine dioxide.
  • Pharmaceutical multipurpose vessels.
  • Hydrofluoric and sulfuric acid service with contaminants.

Alloy 59 or C-276?

In strongly reducing hydrochloric acid, C-276 and especially B-3 can be better; in oxidizing and mixed media alloy 59 usually leads. Choose on corrosion data for the actual medium, not on price alone.

Testing and certification

The A265 certificate reports the chemical analysis of both layers, the Section 7 test results, the bond quality class and any additional tests on the order.

Test or document Basis Frequency / note
Chemical analysis of both layers SA-516 and ASTM B575 Each heat; product analysis (S2) if ordered
Tensile test A265 and the base specification Each plate as rolled
Shear test or three bond bend tests A265 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Corrosion test of cladding Agreed method When ordered
Penetrant test of cladding repairs A265 Section 14 Each repair, reported with location and procedure
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

If your project does not accept weld repairs of the cladding, or wants to approve them first, state that restriction on the order; A265 lists it as a purchaser option.

Equivalent standards and grades

Other standards describe the same product with their own test levels; use them to cross-check, not to substitute without review.

Standard Scope Bond shear requirement
ASTM A265 / ASME SA-265 Nickel and nickel-base alloy-clad steel plate 140 MPa min, when specified
JIS G3602 Nickel and nickel alloy clad steels Per JIS G3602
NB/T 47002.2 Clad plate for pressure equipment, nickel-steel Per NB/T 47002.2
Layer ASTM / ASME UNS EN / W.Nr. JIS GB
Cladding B575 / SB-575 UNS N06059 (alloy 59) UNS N06059 2.4605 (NiCr23Mo16Al) — —
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Chinese projects order nickel-steel clad plate under NB/T 47002.2 and Japanese projects under JIS G3602; confirm that the cladding grade is listed in the edition cited or agree it. Treat these as close equivalents and verify against the design code.

Why order Alloy 59 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying nickel alloy clad plate to FGD, chemical and pharmaceutical fabricators. For alloy 59 clad plate we keep the sheet certificates, including iron, carbon and silicon, with the clad plate report.

  • We check the enquiry against ASTM A265 and flag missing items: cladding specification, bond class, shear test, PWHT simulation.
  • We quote cladding and base thicknesses separately, as minimum or nominal.
  • The nickel alloy sheet and the base plate come with traceable mill certificates; UT maps are supplied when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut to drawing.

FAQ

Is alloy 59 clad plate ordered to ASTM A265?
Yes. A265 (or ASME SA-265) covers nickel-base alloy claddings and lists B575, which includes UNS N06059, among its cladding standards.
How does alloy 59 differ from C-276?
Alloy 59 has more chromium, less iron and no tungsten, so it handles oxidizing and mixed media better and is more thermally stable; C-276 can be better in strongly reducing acids.
Which filler metal is used for alloy 59 clad plate?
ERNiCrMo-13 or ENiCrMo-13, matching alloy 59, in at least two layers with low heat input.
Is alloy 59 used in FGD?
Yes, in the most severe zones such as absorber inlets and outlet ducts.
Is ASME SA-265 the same as ASTM A265?
Yes in content. ASME publishes A265 as SA-265 in Section II Part A, identical with ASTM A265-12(2019). Order SA-265 for ASME Code vessels.
What is the HS code for nickel alloy clad plate?
Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
ASTM A265 or ASME SA-265, Alloy 59 cladding thickness and specification, base grade and thickness, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, and certificate type.

Request a quotation for ASTM A265 SA516 Gr.70 + Alloy 59 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.70 + Alloy 59 nickel alloy clad plate combines B575 alloy 59 with an SA516 Grade 70 base, explosion bonded, with 140 MPa minimum shear when specified and ultrasonic bond quality Class 1, 3 or 5. It is the clad solution for severe mixed acids, FGD and incineration service.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other claddings on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X