ASME SA240 UNS S34565 Stainless Steel Plate
What is ASME SA240 UNS S34565 Stainless Steel Plate?
Equivalent grades: UNS S34565 ≈ EN 1.4565 X2CrNiMnMoN25-18-6-5 ≈ GB/T 022Cr24Ni17Mo5Mn6NbN (S34553).
UNS S34565 is a high-nitrogen super-austenitic grade. S34565 combines 24 % Cr, 4.5 % Mo and about 0.5 % N; manganese is added mainly to keep that much nitrogen in solution. The result is the highest yield strength of the standard austenitic grades in A240 together with a PREN of about 45 or more. Thinner gauges can therefore replace 6Mo or super-duplex plate while keeping a fully austenitic, non-magnetic structure.
ASME SA-240 is the Boiler and Pressure Vessel Code version of ASTM A240, published in Section II Part A. It is ordered when plate will be used in Code construction such as Section VIII pressure vessels, Section I boilers or B31.3 piping components made from plate. Chemistry and tensile limits are the same as in A240, but the certificate and marking must state SA-240 so the Authorized Inspector can accept the material.
This page sets out the ASME SA-240/SA-240M requirements for UNS S34565 plate: specification summary, chemistry, mechanical properties, corrosion resistance, heat treatment, finishes and tolerances, current stock, equivalents, fabrication and testing. SHH STEEL supplies it mill-direct from China with EN 10204 3.1 certificates, optional third-party inspection and in-house cutting.
UNS S34565 plate: specification summary
| Item | UNS S34565 data |
|---|---|
| Standard | ASME BPVC Section II Part A, SA-240/SA-240M (identical with or adapted from ASTM A240/A240M) |
| General requirements | SA-480/SA-480M |
| Product form | plate 5.00 mm (3/16 in.) and over; sheet and strip also covered |
| Typical thickness | 5–80 mm hot-rolled; heavier by mill enquiry |
| Widths | 1500, 2000, 2500 mm; wider by enquiry |
| Lengths | 6000 mm standard; up to 12000 mm or cut to size |
| Finish | No.1 (hot-rolled, annealed and pickled) |
| Marking | SA-240 with grade, heat and plate number; dual A240/SA-240 marking common |
| Certificates | EN 10204 3.1 stating SA-240; 3.2 with third-party or AI witness on request |
| Grade family | super-austenitic |
Size range. Plate is produced on Steckel or reversing mills from about 5 mm up to 80–100 mm depending on grade, with widths of 1500–2500 mm and lengths up to 12 m; thinner plate of 3–12 mm is often cut from hot-rolled coil. Very heavy or wide plates, and plates with tight flatness, should be confirmed before ordering. UNS S34565 is a specialty grade made by a limited number of mills in campaign rolling. Stock covers the common sizes listed below; for project quantities or unusual sizes, plan for a mill campaign and reserve the heat early.
Chemical composition of UNS S34565 (ASME SA-240/SA-240M)
| Element | wt % |
|---|---|
| C | 0.030 max |
| Si | 1.00 max |
| Mn | 5.0–7.0 |
| P | 0.030 max |
| S | 0.010 max |
| Cr | 23.0–25.0 |
| Ni | 16.0–18.0 |
| Mo | 4.0–5.0 |
| N | 0.40–0.60 |
| Nb | 0.10 max |
Single values are maximums unless marked min. Ranges are heat (cast) analysis limits.
PREN check (Cr + 3.3 Mo + 16 N): about 42.6 at the specification minimums and about 46.9 at mid-range. Where corrosion resistance is critical, write a minimum PREN on the order and ask for the calculated value from the heat analysis on the certificate.
Mechanical properties of UNS S34565 plate
| Condition / thickness | Tensile strength, min | Yield strength 0.2 %, min | Elongation in 50 mm, min | Hardness, max |
|---|---|---|---|---|
| all thicknesses | 795 MPa (115 ksi) | 415 MPa (60 ksi) | 35 % | 241 HBW / 100 HRB |
The minimum yield strength of 415 MPa is about 2.4 times the 170 MPa minimum of ASTM 316L. The nitrogen addition is responsible for most of the extra strength; it also increases forming loads compared with 316L. Tension tests are taken in the direction stated in the standard; where a hardness limit is given, it is a maximum that confirms correct annealing.
Corrosion resistance of UNS S34565: PREN and limits
Super-austenitic grades are bought for one reason: chloride resistance. The pitting resistance equivalent number (PREN = Cr + 3.3 Mo + 16 N) at the specification minimum is about 42.6, and a mid-range heat is about 46.9. In practice this means resistance to pitting and crevice attack in seawater and chloride process streams where 316L and 904L fail, and a critical pitting temperature (ASTM G48 Method C/E) that is usually well above 50 °C for good mill product.
Because the structure is fully austenitic, these steels are also immune to the 300 °C service limit that applies to duplex, they stay tough at cryogenic temperatures, and they do not need ferrite control. The trade-off is segregation: high molybdenum segregates during solidification and can form sigma and chi phases if plate is cooled slowly after solution annealing. Good practice is to specify an ASTM G48 or A262-type acceptance test on the actual heat and to ask for the solution-anneal temperature on the mill certificate.
How UNS S34565 compares with related grades
| Grade | Cr | Ni | Mo | N | PREN (min) | YS / Rp0.2 min, MPa |
|---|---|---|---|---|---|---|
| UNS S34565 | 23.0–25.0 | 16.0–18.0 | 4.0–5.0 | 0.40–0.60 | 42.6 | 415 |
| UNS S31254 | 19.5–20.5 | 17.5–18.5 | 6.0–6.5 | 0.18–0.25 | 42.2 | 310 |
| UNS N08367 | 20.0–22.0 | 23.5–25.5 | 6.0–7.0 | 0.18–0.25 | 42.7 | 310 |
| UNS S32654 | 24.0–25.0 | 21.0–23.0 | 7.0–8.0 | 0.45–0.55 | 54.3 | 430 |
Choose UNS S34565 for warm seawater, chloride process streams and acidic chloride service where a fully austenitic, tough and non-magnetic structure is preferred. It costs more than super duplex in most markets, so it is usually chosen where low-temperature toughness, formability or service above 300 °C rules duplex out.
The table uses specification limits, not typical mill values, so it shows the guaranteed position of each grade. Final selection should also consider product availability in the thickness you need, welding consumables, and the inspection requirements of your project.
Heat treatment and delivery condition of UNS S34565
Heat treatment: 1120–1170 °C, rapid cooling.
A high solution-anneal temperature dissolves sigma and chi phases and evens out molybdenum segregation; water quenching is used for plate. Hot forming should finish above about 1000 °C and be followed by a solution anneal.
Surface finishes for UNS S34565 plate
Plate to SA-240 is normally supplied with a No.1 finish: hot rolled, solution annealed and pickled, with a matt grey surface. Shot-blasted and pickled surfaces are the norm on heavy plate. Ground or polished faces, and plates with protective film for the process side, can be produced after delivery in our workshop. Surface defects are judged against the A480/SA-480 workmanship clause; for vessel internals the purchaser may add surface-roughness or cleanliness requirements.
Dimensions, tolerances and flatness
Thickness, width, length, flatness and camber tolerances follow SA-480/A480 tables for hot-rolled plate; ordered thickness is a minimum unless the order states nominal. For pressure parts, the thickness at any point must not fall below the ordered minimum, so heavy plate is often ordered with a small plus allowance. Flatness of thin plate cut from coil should be checked after cutting. Mill edge, sheared, plasma or waterjet-cut edges and bevelling for welding are available.
Code use of SA-240 plate. Before welding, the manufacturer must identify the P-Number and group number of S34565 from ASME Section IX (QW/QG-422) for the welding procedure qualification, and the designer takes allowable stresses from Section II Part D. Impact-test exemptions for austenitic and duplex plate are given in Section VIII Division 1 (UHA-51) and depend on grade, thickness and minimum design metal temperature, so cryogenic or low-temperature duty should be stated when you order. For heavy plate, ultrasonic examination to SA-578 and PMI of each plate are common supplementary requirements. Ask for the plate number to be hard-stamped or stencilled so traceability survives cutting.
UNS S34565 plate stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Finish | Approx. quantity | Location |
|---|---|---|---|---|---|
| 6 | 1500 / 2000 | 6000 | No.1 | 100+ t | China |
| 8 | 1500 / 2000 | 6000 | No.1 | 100+ t | China |
| 10 | 2000 | 6000 | No.1 | 100+ t | China |
| 12 | 2000 | 6000 | No.1 | 100+ t | China |
| 16 | 2000 / 2500 | 6000 | No.1 | 100+ t | China |
| 20 | 2000 / 2500 | 6000 / 8000 | No.1 | 100+ t | China |
| 30 | 2000 / 2500 | 6000 | No.1 | 100+ t | China |
Quantities are approximate and stock changes daily. Send your size list for current availability; other thicknesses, widths and cut sizes can be supplied from mill production.
Packing and logistics. Plate is bundled on steel or wooden skids with steel bands and edge protection, typically 3–8 t per bundle, and marked with heat and plate numbers. Cut pieces are crated. Heavy and wide plate ships in open-top or flat-rack containers or by break-bulk; we send loading photos with the shipping documents.
UNS S34565 equivalents in other standards
| Standard | Designation | Comment |
|---|---|---|
| EN | 1.4565 X2CrNiMnMoN25-18-6-5 | same alloy family and limits closely matched; compare each limit on the certificate |
| GB/T | 022Cr24Ni17Mo5Mn6NbN (S34553) | same alloy family and limits closely matched; compare each limit on the certificate |
Equivalents are close, not identical. When a project names one standard, order to that standard or ask for multiple certification and check every limit on the certificate.
Related grades by alloy family
Super austenitic
6Mo and 7Mo grades for seawater and chloride service; upgrade path from 316L and 904L: SA-240 N08904, SA-240 S31726, 1.4547 plate, 1.4529 plate, 1.4539 plate, SA-240 S31254, SA-240 N08367, SA-240 S32654.
Super duplex
PREN 40+ duplex grades for seawater and severe chlorides: SA-240 S32750, 1.4410 plate, 1.4501 plate, 1.4507 plate.
Same grade, other specification
Applications, forming and welding of UNS S34565
Typical uses: seawater and brine equipment, FGD and chemical-plant vessels, offshore and marine structures where non-magnetic properties are needed, and pressure equipment that benefits from high allowable stress.
In fabrication, plate cuts and forms like heavy austenitic plate but needs higher bending forces because of the nitrogen. Cut by plasma, laser or waterjet and remove heat tint by pickling or grinding. For welding use an over-alloyed nickel-base filler such as ERNiCrMo-3 or ERNiCrMo-13 (AWS A5.14), because a matching filler would lose molybdenum to segregation in the weld. Keep the weld area clean and free of carbon-steel contamination, and pickle and passivate after welding where corrosion resistance matters.
Welding practice. Weld with low to moderate heat input and interpass temperature below about 100 °C. An over-alloyed nickel-base filler compensates for molybdenum segregation in the weld metal; autogenous welds lose much of the base-metal pitting resistance and should be avoided on wetted surfaces unless the weld is solution annealed afterwards. Pickling after welding is essential to restore the passive layer.
Certificates, testing and receiving inspection
Every delivery carries a mill certificate to ASME SA-480/SA-480M with heat analysis, tensile results and hardness, and the grade and standard as ordered. Supplementary tests we can arrange: ASTM G48 Method A or critical pitting temperature (Method C/E), ASTM A262 practice where specified, microstructure check for sigma/chi, ultrasonic testing of plate, and PMI. Third-party witness by SGS, BV, TÜV, DNV, ABS or LR is available with EN 10204 3.2 certificates.
On receipt, check marking and heat number against the certificate, measure thickness at several points and confirm the finish and edge condition before cutting.
Common mistakes when specifying UNS S34565
- Ordering by trade name instead of the UNS or EN number, which leaves chemistry open.
- Welding with matching filler on seawater-wetted surfaces.
- Skipping a corrosion acceptance test on heavy plate where segregation is most likely.
Each of these can be avoided by writing the requirement into the purchase order and checking it on the certificate before the material is cut.
Sourcing UNS S34565: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Segregation and sigma in thick plate | solution-anneal temperature and quench recorded; G48 or CPT test on the actual heat |
| Long mill lead times | stock plate checked first; heats reserved early for project quantities |
| Small quantities across many sizes | mixed thicknesses and grades combined in one shipment |
| Cutting and edge preparation | in-house shearing, plasma, laser and waterjet cutting, bevelling |
| Delivery delays | weekly production and shipping updates with photos |
How to order UNS S34565 plate
State the standard and edition (ASME SA-240/SA-240M), the grade (UNS S34565), thickness, width and length or coil, finish, quantity, tolerance class, any added chemistry limits, the supplementary tests and acceptance values from your specification, the certificate type and inspection agency, and packing. Send the list to SHH STEEL and we will reply with price, available stock and lead time.
FAQ
-
What is the difference between SA-240 and A240 for S34565?
- The chemistry and tensile requirements are the same. SA-240 is the ASME Code edition, so plate for pressure vessels must be certified and marked SA-240; dual-certified A240/SA-240 plate covers both.
-
Is UNS S34565 equivalent to EN 1.4565 X2CrNiMnMoN25-18-6-5?
- They are the same alloy designation in different standards. Limits are closely matched, but always order to the standard named in your specification or ask for multiple certification.
-
Is UNS S34565 better than super duplex in seawater?
- Both are used in seawater. Super-austenitic grades are fully austenitic, tough at low temperature and not limited to about 300 °C, while super duplex has higher strength. The choice depends on temperature, chlorination and design stress.
-
Can I order small quantities or cut sizes?
- Yes. We combine mixed thicknesses and grades into one shipment and cut plate and sheet to size in our workshop.
-
Which certificates and tests can you provide?
- Every order ships with a mill certificate (EN 10204 3.1 type) showing heat analysis and mechanical tests. Supplementary tests and 3.2 certificates with SGS, BV, TÜV or another agency are available by agreement.
Conclusion
UNS S34565 plate should be ordered with the points the standard leaves open written into the contract: finish, tolerance class, any extra chemistry limits and the supplementary tests your application needs. With those fixed, stock material from China is a fast and reliable route.