JIS G 3101 SS540 Steel Channel

JIS G 3101 SS540 steel channel is a general-structure section named for a 540 N/mm² tensile minimum, not for a 540 N/mm² yield. Yield is 400 N/mm² up to 16 mm and 390 N/mm² between 16 mm and 40 mm, based on flange thickness t2. Mechanical properties stop at 40 mm. Dimensions follow the JIS G 3192 Table 12 channel series. This page is SS540 only, not SS400, SS490 or SM490. SHH STEEL reviews grade, designation, edition and certificate requirements before quoting.
Keywords
JIS G 3101 SS540 Steel Channel, SS540 channel, SS540 JIS G 3192 channel, 540 N/mm² structural channel, Japanese steel channel
Equivalent Grades:
Near-equivalents only, not automatic substitutes: SS490 and SS400 are lower-tensile grades in the same standard; SM490 is a different JIS standard (G 3106); A572 Grade 50 is a different specification and shape system; Q355B; S355JR.
Share:
General Description
Material Specification
Available Sizes of SS540 Steel Channel
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why Source SS540 Steel Channels from SHH STEEL
FAQ
Conclusion

What is JIS G 3101 SS540 Steel Channel?

JIS G 3101 SS540 steel channel is a hot-rolled channel in rolled steel for general structure, grade SS540. The material standard is JIS G 3101, Rolled steels for general structure. The chemical and mechanical figures on this page are those of the issued JIS G 3101:2015 tables. JIS G 3101:2024 is the current listed edition, issued 20 February 2024; the edition named on the order governs acceptance. Dimensions, mass and tolerances for the section itself are those of JIS G 3192:2024. SHH STEEL supplies these channels to the grade, designation, edition and certificate named on the order.

The number in the grade name is the specified tensile strength in N/mm² (1 N/mm² = 1 MPa), not a yield class. Formal grades in the standard are SS330, SS400, SS490 and SS540. This page is SS540. It is not the JIS G 3101 SS400 steel channel page, not SS490, not a JIS G 3106 SM490 steel channel, and not a data sheet for SS540 steel plate.

The standard designation is the four-part size H×B×t1×t2, for example 150×75×6.5×10 or 380×100×13×20, where H is the depth, B the flange width, t1 the web thickness and t2 the flange thickness. The designation is not an American C or MC prefix, and a 200 mm Japanese channel is not a UPN 200, a UPE 200 or a Chinese channel of similar depth.

SS540 chemistry is tighter than the SS400/SS490 row: Table 2 gives carbon 0.30% max and manganese 1.60% max, with phosphorus and sulfur 0.040% max. Mechanical properties in Table 3 stop at 40 mm. Every standard Table 12 flange on this page is at or below 20 mm, so all tabulated rows are inside that cap.

These channels are filed under JIS G3101 steel channel profiles in the steel channel profiles category of steel structural profiles. The same grade in plate form is listed separately; do not use a plate page as a channel data sheet.

SS540 channels are used for building and general industrial framing when the specification names this higher-tensile G 3101 grade. JIS G 3101 does not specify a Charpy test for SS540. The grade is not a pressure-vessel or nuclear safety material, and it is not a substitute for JIS G 3106 SM490 when a welded-structure grade and a defined impact quality are what the order requires.

Material, Dimensions and Tolerances for SS540 Channels

Keep the material specification and the dimensional standard distinct. JIS G 3101 is the material standard. The ladle-analysis and mechanical figures used here are those of the issued JIS G 3101:2015 tables (Table 2 and Table 3), and the mechanical table for SS540 stops at 40 mm, in line with Table 1. JIS G 3101:2024 is the current listed edition; the edition named on the order governs acceptance. JIS G 3192:2024 is the shape standard for these channels. A documented special combination is valid only if every requirement of each named standard is met. Matching a nominal 200 mm or 8 in depth is not a substitution method. JIS G 3101 does not require a fully killed practice and does not require the product to be normalized.

SS540 Channel Sizes: JIS G 3192 Standard Channel Series

The table lists the 16 standard channel sizes in JIS G 3192:2024 Table 12, with designation H×B×t1×t2, the tabulated root and toe radii r1 and r2, theoretical area and theoretical mass. Use the table to identify and estimate, not as a rolling programme for SS540. Mid-range sizes such as 150×75 and 200×90 are the usual enquiry core; the 75×40 row and the 380×100 rows should be confirmed size by size.

The tabulated sizes are the complete standard series in Table 12. They are representative dimensions; other section dimensions may be used by agreement between the parties, but this page does not invent rows that Table 12 does not list. SS540 mechanical properties stop at 40 mm; every Table 12 flange on this page is at or below 20 mm, so all tabulated rows are inside that cap.

75×40×5×7 has a 7 mm flange, so the 400 N/mm² yield band applies. 300×90×12×16 has a 16 mm flange and remains in that first band. 380×100×13×16.5 and 380×100×13×20 have 16.5 mm and 20 mm flanges, so the minimum yield is 390 N/mm², not 400 N/mm². 150×75×6.5×10 and 150×75×9×12.5 share the same depth and flange width but are different sections.

16 standard sizes, from 75×40×5×7 to 380×100×13×20.

Swipe horizontally to view all dimensions.

Designation (H×B×t1×t2) H (mm) B (mm) t1 (mm) t2 (mm) r1 (mm) r2 (mm) A (cm²) Mass (kg/m)
75×40×5×7 75 40 5 7 8 4 8.818 6.92
100×50×5×7.5 100 50 5 7.5 8 4 11.92 9.36
125×65×6×8 125 65 6 8 8 4 17.11 13.4
150×75×6.5×10 150 75 6.5 10 10 5 23.71 18.6
150×75×9×12.5 150 75 9 12.5 15 7.5 30.59 24.0
180×75×7×10.5 180 75 7 10.5 11 5.5 27.20 21.4
200×80×7.5×11 200 80 7.5 11 12 6 31.33 24.6
200×90×8×13.5 200 90 8 13.5 14 7 38.65 30.3
250×90×9×13 250 90 9 13 14 7 44.07 34.6
250×90×11×14.5 250 90 11 14.5 17 8.5 51.17 40.2
300×90×9×13 300 90 9 13 14 7 48.57 38.1
300×90×10×15.5 300 90 10 15.5 19 9.5 55.74 43.8
300×90×12×16 300 90 12 16 19 9.5 61.90 48.6
380×100×10.5×16 380 100 10.5 16 18 9 69.39 54.5
380×100×13×16.5 380 100 13 16.5 18 9 78.96 62.0
380×100×13×20 380 100 13 20 24 12 85.71 67.3

SS540 Chemical Composition for Channels (Table 2)

The ladle analysis shall comply with Table 2 of JIS G 3101, using the issued 2015 figures given below. JIS G 3101:2024 is the current listed edition; the edition named on the order governs. Unlike SS400 and SS490, the SS540 row specifies carbon and manganese as well as phosphorus and sulfur.

Element SS540 ladle analysis, Table 2 (mass %)
C, max 0.30
Mn, max 1.60
P, max 0.040
S, max 0.040

These are maxima, not typical heat results, and they are not an invitation to describe the grade as “containing 0.30% carbon and 1.60% manganese.” Alloying elements not listed in Table 2 may be added as necessary. Table 2 is a ladle-analysis table. The issued 2015 text recovered for this page specifies ladle analysis only and does not give a separate numeric product-analysis table. This page does not invent one.

SS540 Channel Mechanical Properties: Yield, Tensile and Elongation

Mechanical properties of SS540 plates, strip, flats and sections follow Table 3 of the issued JIS G 3101:2015 text, and they stop at 40 mm, in line with Table 1. These channels use the plate, strip, flat and section rows of that table, not the bar rows. The recovered 2015 Table 3 notes do not add an upper-yield or 0.2% proof-stress instruction, and this page does not add one. Thickness for a section is the thickness at the test-piece location; on this page the usual basis for selecting a yield band is the flange thickness t2.

Property Table 3 requirement for SS540 sections
Minimum yield, t ≤ 16 mm 400 N/mm²
Minimum yield, 16 mm < t ≤ 40 mm 390 N/mm²
Tensile strength 540 N/mm² minimum (no tabulated maximum)
Elongation, t ≤ 5 mm 16% min, test piece No. 5
Elongation, 5 mm < t ≤ 16 mm 13% min, test piece No. 1A
Elongation, 16 mm < t ≤ 40 mm 17% min, test piece No. 1A
Bend 180°, inner radius 2.0 × thickness, test piece No. 1 (No. 3 may be used at 5 mm and under)

There is no Table 3 yield or elongation band above 40 mm for SS540, and this page does not invent one. JIS G 3101 does not specify Charpy absorbed-energy values. The bend test may be omitted unless the purchaser specifies it; the steel still has to satisfy the bendability requirement, and the outside of the bend piece must be free of cracks.

Delivery, Inspection and Identification of SS540 Channels

SS540 channels are commonly supplied as-rolled. If not otherwise specified at the time of order, the default inspection document is a JIS G 0415 inspection certificate 3.1. The document should identify JIS G 3101 and its edition, the grade SS540, the G 3192 designation, the heat number, the ladle analysis and the tensile results. An EN 10204 type 3.1 request is usually satisfied by that 3.1 document; type 3.2 or nominated third-party attendance can be added when the order requires it. Length is a matter for the rolling programme and the order, often in the region of 6–12 m; those lengths are enquiry ranges, not a stock list. A SS540 plate certificate does not identify a channel.

Weldability and Surface Condition of SS540 Channels

SS540 is a general structural steel intended to be welded, bolted or otherwise fabricated when the procedure is suitable for the thickness and the joint. JIS G 3101 does not table a carbon-equivalent limit or a Charpy value for this grade. This page does not prescribe a welding procedure or a preheat chart. The as-rolled surface is mill scale. Blast, paint or galvanizing is an order option. Cutting, punching, forming or coating can be reviewed when that specification is sent with the enquiry.

JIS G 3192 Shape Tolerances and Theoretical Mass

Dimensional and mass tolerances for these channels are those of JIS G 3192, not of JIS G 3101 itself. This article does not reproduce the millimetre tolerance tables; acceptance is against the edition of G 3192 named on the order. Root and toe radii in the tables are tabulated standard dimensions in this series. Settlement on theoretical or weighed mass should follow the contract.

Applications and Service Limits

SS540 steel channels are used where a general structural L-section in this tensile class is specified: frames, bracing, towers, shops and fabrications that name JIS G 3101 SS540 rather than SS400, SS540 or a welded-structure grade such as SM490. The grade is not specified here as a pressure-vessel or nuclear-safety material. Durability comes from the coating or fire-protection system named on the order, not from the SS540 designation itself.

SS540 Channel Compared with SS400, SS490 and Other 50 ksi-Class Grades

JIS G 3101 SS400 steel channel uses the same G 3192 Table 12 series at a much lower tensile range (400–510 N/mm²) and a lower yield band (245 N/mm² up to 16 mm). An SS400 certificate is not an SS540 certificate.

SS490, also in JIS G 3101, has a 490–610 N/mm² tensile range and a 285/275 N/mm² yield band. It also shares the looser Table 2 chemistry row (phosphorus and sulfur only). It is a related grade, not this data sheet.

JIS G 3106 SM490 steel channel also uses the G 3192 channel series, but SM490 is a welded-structure grade under a different standard. Do not treat a 50 ksi-class comparison as a substitute certificate.

Near-Equivalents: Not Automatic Substitutes

The comparisons above are for orientation. They are not a licence to substitute one grade, one certificate or one shape system for another. SS540 chemistry is C 0.30 max, Mn 1.60 max, with tighter P and S. Use the sister pages for their own standards.

Stock and Supply of SS540 Steel Channels from SHH STEEL

SHH STEEL supplies JIS G 3101 SS540 steel channels as an export trading house, coordinating mill production and project procurement. The useful work on this product is to keep SS540 distinct from SS400 and SS490 and from JIS G 3106 grades, to select the correct yield band from the flange thickness, to respect the 40 mm mechanical cap, and to align the G 3192 designation, the edition and the inspection document before a rolling programme is committed.

Sizes, lengths and certificates are confirmed per enquiry. The table is the standard G 3192 Table 12 series, not a list of pieces on the floor. Mid-range 150×75 and 200×90 sizes are the usual core; the 75×40 row and the 380×100 rows are confirmed per line.

Sections can be sourced from mills that SHH STEEL buys from, including Masteel, Rizhao Steel, Laiwu (Shandong Steel Laiwu) and Tung Ho Steel, among others when the programme matches the order. Those mills do not each roll every Table 12 size in SS540. If cutting, punching, forming or a coating system is required, include that specification for review. Export packing and container loading can be arranged to the packing list agreed for the shipment.

SS540 Steel Channel FAQs

Is SS540 a 540 N/mm² yield grade?
No. The 540 in the grade name is the specified tensile minimum (no tabulated maximum). Minimum yield is 400 N/mm² for flange thickness up to 16 mm, and 390 N/mm² between 16 mm and 40 mm. Do not read the grade number as a yield class.
Can I order SS540 thicker than 40 mm?
Not under the Table 3 mechanical rows used on this page. SS540 mechanical properties stop at 40 mm. Every standard JIS G 3192 Table 12 flange tabulated here is at or below 20 mm, so those rows are inside the cap. A thicker special would need its own agreement; this page does not invent a band above 40 mm.
Is an SS490 channel automatically acceptable as SS540?
No. They share the same G 3192 Table 12 series, but SS540 has a higher tensile minimum, a higher yield band, and a tighter chemistry row (carbon and manganese maxima). An SS490 certificate is not an SS540 certificate.
Which thickness is used to pick the yield band?
Thickness for a section is the thickness at the test-piece location. On this page the usual basis is the flange thickness t2, not the channel depth H. A 380×100 channel with a 16.5 mm or 20 mm flange uses the 390 N/mm² band, not the 400 N/mm² band.
Does JIS G 3101 require a Charpy test for SS540?
No. JIS G 3101 does not specify Charpy absorbed-energy values for SS540. If an impact test is required, it has to be named on the order.

Request a Quotation for JIS G 3101 SS540 Steel Channel

JIS G 3101 SS540 steel channel is a general-structure section with a 540 N/mm² tensile minimum and 400 N/mm² minimum yield up to 16 mm (390 N/mm² between 16 mm and 40 mm, based on flange thickness). Mechanical properties stop at 40 mm. Nominate the JIS G 3192 channel size (H×B×t1×t2) and the material to JIS G 3101:2024 (or the edition on the order). The table is the standard Table 12 series, used as reference dimensions, not a rolling list. Send the size list, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X