JIS G 3101 SS400 Steel Channel

JIS G 3101 SS400 steel channel is a general-structure channel named for a 400–510 N/mm² tensile range, not a 400 N/mm² yield. Minimum yield is 245 N/mm² up to 16 mm. Dimensions follow the JIS G 3192 standard channel series. The ordered edition governs. SHH STEEL reviews grade, designation, edition and certificate requirements before quoting.
Keywords
JIS G 3101 SS400 Steel Channel, SS400 channel, JIS G 3192 channel, SS400 mizo-gata channel, general-structure channel
Equivalent Grades:
Near-equivalents only, not automatic substitutes: Q235B; S235JR; SM490A and SM490B belong to JIS G 3106 and are not SS400 certificates.
Share:
General Description
Material Specification
Available Sizes of SS400 Steel Channel
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why Source SS400 Steel Channels from SHH STEEL
FAQ
Conclusion

What is JIS G 3101 SS400 Steel Channel?

JIS G 3101 SS400 steel channel is a hot-rolled channel in rolled steel for general structure, grade SS400. The material standard is JIS G 3101. Dimensions, mass and tolerances for the section itself are those of JIS G 3192. The “400” in the grade name is the lower end of the specified tensile range (400–510 N/mm²). It is not a 400 N/mm² yield. Up to 16 mm, the minimum yield point or proof stress is 245 N/mm², and it steps down as the thickness at the test-piece location increases.

The standard designation is the four-part size H×B×t1×t2, for example 150×75×6.5×10 or 380×100×13×20, where H is the depth, B the flange width, t1 the web thickness and t2 the flange thickness. The standard allows thickness to be shown as t1 only, but this page lists both thicknesses because several depths share the same H and B with more than one t1×t2 combination. The designation is not an American C or MC prefix, and a 200 mm Japanese channel is not a UPN 200, a UPE 200 or a Chinese channel of similar depth.

These channels are filed under JIS G3101 steel channel profiles in the steel channel profiles category of steel structural profiles. The same grade in plate form is listed separately as JIS G 3101 SS400 steel plate. Do not use that plate page as a channel data sheet, and do not copy a plate elongation-reduction rule onto a channel certificate.

SS400 channels are used for building and general industrial framing when the specification names this Japanese general-structure grade. JIS G 3101 does not specify a Charpy test for SS400. The grade is not a pressure-vessel or nuclear safety material, and it is not a substitute for JIS G 3106 SM490 when a welded-structure grade and a defined impact quality are what the order requires.

Material, Dimensions and Tolerances for SS400 Channels

The order and the inspection certificate should keep material, dimensions and tolerances distinct:

  • JIS G 3101 is the material standard. This article uses heat-analysis and tensile values for SS400 from JIS G 3101:2024. The edition named on the order governs acceptance.
  • JIS G 3192 is the dimensional, mass and tolerance standard for these hot-rolled channels. The size table below is the complete standard channel series in JIS G 3192:2024 Table 12. The tabulated sizes are representative; other section dimensions may be used by agreement. The edition of JIS G 3192 named on the order governs dimensional and mass acceptance.

A documented special combination — for example SS400 on a European UPN, or a JIS channel certified to a different material standard — is only valid if every requirement of each named standard is met. Matching a nominal 200 mm or 8 in depth is not a substitution.

SS400 Channel Sizes: JIS G 3192 Standard Channel Series

The table lists the 16 standard channel sizes in JIS G 3192:2024 Table 12, with designation H×B×t1×t2, the tabulated root and toe radii r1 and r2, theoretical area and theoretical mass. Use the table to identify and estimate, not as a rolling programme for SS400. Mid-range sizes such as 150×75 and 200×90 are the usual enquiry core; the 75×40 row and the 380×100 rows should be confirmed size by size.

The tabulated sizes are the complete standard series in Table 12. They are representative dimensions; other section dimensions may be used by agreement between the parties, but this page does not invent rows that Table 12 does not list.

75×40×5×7 has a 7 mm flange, so the 245 N/mm² yield band applies. 300×90×12×16 has a 16 mm flange and remains in that first band. 380×100×13×16.5 and 380×100×13×20 have 16.5 mm and 20 mm flanges, so the minimum yield is 235 N/mm², not 245 N/mm². 150×75×6.5×10 and 150×75×9×12.5 share the same depth and flange width but are different sections.

16 standard sizes, from 75×40×5×7 to 380×100×13×20.

Swipe horizontally to view all dimensions.

Designation (H×B×t1×t2) H (mm) B (mm) t1 (mm) t2 (mm) r1 (mm) r2 (mm) A (cm²) Mass (kg/m)
75×40×5×7 75 40 5 7 8 4 8.818 6.92
100×50×5×7.5 100 50 5 7.5 8 4 11.92 9.36
125×65×6×8 125 65 6 8 8 4 17.11 13.4
150×75×6.5×10 150 75 6.5 10 10 5 23.71 18.6
150×75×9×12.5 150 75 9 12.5 15 7.5 30.59 24.0
180×75×7×10.5 180 75 7 10.5 11 5.5 27.20 21.4
200×80×7.5×11 200 80 7.5 11 12 6 31.33 24.6
200×90×8×13.5 200 90 8 13.5 14 7 38.65 30.3
250×90×9×13 250 90 9 13 14 7 44.07 34.6
250×90×11×14.5 250 90 11 14.5 17 8.5 51.17 40.2
300×90×9×13 300 90 9 13 14 7 48.57 38.1
300×90×10×15.5 300 90 10 15.5 19 9.5 55.74 43.8
300×90×12×16 300 90 12 16 19 9.5 61.90 48.6
380×100×10.5×16 380 100 10.5 16 18 9 69.39 54.5
380×100×13×16.5 380 100 13 16.5 18 9 78.96 62.0
380×100×13×20 380 100 13 20 24 12 85.71 67.3

SS400 Chemical Composition for Channels (JIS G 3101 Heat Analysis)

The figures below are heat-analysis limits for SS400 in JIS G 3101:2024. They should not be copied from SS540, which does have carbon and manganese maxima, or from a Chinese or European 235 MPa table that publishes carbon and manganese limits SS400 does not. They are limits, not typical heat results.

Element Heat analysis, max (mass %) Notes for SS400 channels
C No tabulated maximum The carbon column for SS400 is a dash, not a zero-carbon requirement. Carbon and other unlisted elements may be added as necessary, and if they are added they shall be reported.
Mn No tabulated maximum The manganese column for SS400 is also a dash. Do not copy an SS540 manganese maximum (1.60%) onto an SS400 order.
Si Not a tabulated column JIS G 3101:2024 Table 2 does not list a silicon maximum for SS330, SS400 or SS490.
P 0.050 This is a heat-analysis maximum, not a typical result.
S 0.050 This is a heat-analysis maximum, not a typical result.

SS400 Channel Mechanical Properties: Yield, Tensile, Elongation and Bend

Tensile properties of SS400 sections follow Table 3 of JIS G 3101:2024 (plates, strips, flats and sections). Thickness is that at the test-piece location. For these channels that location is ordinarily the flange thickness t2, not the overall depth H. Unless otherwise specified, the yield value is the upper yield point (ReH); if no yield point appears, 0.2% proof stress (Rp0.2) is determined. Annex JA, which applies to sections with a leg length under 40 mm, is not used for the standard channels in the size table above, whose flange widths are 40 mm or more.

Thickness at the test-piece location (mm) Minimum yield point or proof stress (N/mm²) Tensile strength (N/mm²)
t ≤ 16 245 400–510
16 < t ≤ 40 235 400–510
40 < t ≤ 100 215 400–510
t > 100 205 400–510

Elongation uses the test pieces named in the same table. For No. 4 test pieces on plates thicker than 90 mm, the standard reduces the tabulated elongation by 1 for each 25 mm or fraction of thickness, with a maximum reduction of 3; that reduction is a plate rule and is not extended here to invent a section value. None of the tabulated channel flanges exceeds 20 mm, so the No. 4 band does not arise on the sizes above.

Thickness (mm) Test piece Minimum elongation (%)
t ≤ 5 No. 5 21
5 < t ≤ 16 No. 1A 17
16 < t ≤ 40 No. 1A 21
40 < t ≤ 50 No. 1A 21
t > 50 No. 4 23

The specified bend is 180° with an inner radius of 1.5 times the thickness, using a No. 1 test piece (a No. 3 piece may be used at 5 mm and under). The bend test may be omitted unless the purchaser specifies it, but the steel still has to satisfy the bendability requirement. JIS G 3101 does not specify a Charpy test for SS400; a toughness value must not be inferred from the grade name. If the specification needs a defined impact test, a JIS G 3106 quality such as SM490B or SM490C, or another standard that actually tables that test, should be nominated.

Delivery Conditions, Inspection and Identification

SS400 channels are commonly supplied as-rolled. The inspection document should show JIS G 3101 and its edition, the grade SS400, the JIS G 3192 size designation (H×B×t1×t2), the delivery condition, the heat number, the heat analysis (including any added elements), and the tensile results by thickness. If not otherwise specified at the time of order, the inspection document is a JIS G 0415 inspection certificate 3.1. A toughness result cannot be inferred from an SS400 certificate. A plate certificate, or an H-section certificate, does not, by itself, identify a channel.

Identification follows the mill’s marking practice. Length is a matter for the rolling programme and the order.

Weldability and Surface Condition of SS400 Channels

SS400 is widely welded in general-structure work when thickness, joint design and hydrogen control are taken into account. Because the grade does not publish carbon or manganese maxima, the heat analysis on the certificate, rather than an assumed CEV table, is the practical starting point. This page does not prescribe a procedure or a preheat chart, and it does not invent a carbon-equivalent limit that JIS G 3101 does not table for SS400.

Cutting, punching, forming, blast, paint or galvanizing can be reviewed when that specification is sent with the enquiry. They are not assumed for every size.

JIS G 3192 Shape Tolerances and Theoretical Mass

Dimensional, shape and mass tolerances for these channels are those of JIS G 3192, not of JIS G 3101. This article uses JIS G 3192:2024 as the known edition and does not reproduce the millimetre tolerance tables; acceptance is against the edition named on the order.

A delivered 200×90×8×13.5 will measure close to the tabulated depth, flange and thicknesses within those tolerances, not as a set of exact advertised millimetres. Out-of-square and flange tilt matter for connections. Settlement on theoretical or weighed mass should follow the contract. Theoretical masses in the size table are the tabulated values; they are not a substitute for a weighed-mass agreement if the order requires one.

Applications and Service Limits

SS400 steel channels are used where this Japanese general-structure grade and a JIS G 3192 channel are specified:

  • Building and industrial frames, bracing, stair stringers and general fabrications whose specification names SS400 channel rather than a welded-structure grade or a European or American channel series.
  • Export packages that compare the grade with Q235B or with S235JR plate, provided each line keeps its own material standard and shape system.

It is not specified here for pressure equipment, for nuclear safety-related components, or for members that actually require a defined Charpy test. Durability comes from the coating or fire-protection system, not from the SS400 designation.

SS400 Channel Compared with Q235B, S235JR and SM490

SS400, Q235B and S235JR are often grouped in a 235 MPa discussion, but they are not interchangeable certificates. SS400 is named for its 400–510 N/mm² tensile range and does not publish carbon or manganese maxima, nor a Charpy test. Q235B is a Chinese 235 MPa grade on a different shape system. S235JR plate carries tabulated carbon and manganese and a +20 °C impact test; a European channel in that grade would be a UPN, UPE or PFC, not a JIS G 3192 designation. SS400 plate is the same grade in plate form, not a channel.

SM490A and SM490B can use the same JIS channel series, but they belong to JIS G 3106, with a higher tensile class and, for B and C, specified impact tests. Dual certification requires every requirement of each named standard to be met on the delivered piece. An SS400 H-beam page in this series will be linked here once it is published; that product URL is not pre-linked.

Near-Equivalents: Not Automatic Substitutes

The comparisons below are for orientation. They are not a licence to substitute one grade or one shape for another on a contract or an inspection certificate.

Grade / designation Standard Relationship to SS400 channel Caution
Q235B GB/T 700; dimensions GB/T 706 for channels A common Chinese 235 MPa comparison used in export enquiries, often discussed alongside SS400. Q235B has its own chemistry table, including tabulated carbon and manganese limits that SS400 does not publish. The shape names follow GB/T 706, not the JIS G 3192 H×B×t1×t2 designation.
S235JR EN 10025-2; dimensions EN 10365 A 235 MPa European general-structure comparison, usually as UPN, UPE or PFC when the product is a channel. S235JR has tabulated carbon, manganese and a +20 °C impact test. Those requirements are not implied by an SS400 certificate, and a UPN or UPE is not a JIS channel of similar depth.
SM490A / SM490B JIS G 3106; the same JIS G 3192 channel series may be used Welded-structure grades in a higher tensile class, with specified impact tests for B and C. SM490 is not SS400. An SS400 certificate does not carry a JIS G 3106 impact quality. Dual certification requires every requirement of each named standard to be met on the delivered piece.

Sourcing SS400 Steel Channels from SHH STEEL

SHH STEEL supplies SS400 steel channels as an export trading house, coordinating mill production and project procurement. For this grade the useful work is to keep the tensile-named SS400 designation from being read as a 400 N/mm² yield, to keep the full H×B×t1×t2 designation from being shortened until two rows collide, to apply the yield band to the flange thickness rather than the channel depth, and to align the inspection document with the edition named on the order before a rolling programme is committed.

Sections can be sourced from mills that SHH STEEL buys from, including Masteel, Rizhao Steel, Laiwu (Shandong Steel Laiwu) and Tung Ho Steel, among others when the programme matches the order. Those mills do not each roll every Table 12 size in SS400. Mid-range 150×75 and 200×90 sizes are the usual core; the 75×40 row and the 380×100 rows are confirmed per line.

The same enquiry can also cover H-sections, angles, or Chinese, European or American designations, provided each line states its material standard, shape standard and size. If cutting, punching, forming or a coating system is required, include that specification for review. Export packing and container loading can be arranged to the packing list agreed for the shipment.

SS400 Steel Channel FAQs

Does SS400 have a 400 N/mm² yield?
No. The 400 in the grade name is the lower end of the 400–510 N/mm² tensile range. The minimum yield point or proof stress is 245 N/mm² up to 16 mm, then 235, 215 and 205 N/mm² in the thicker bands. For these channels the governing thickness is ordinarily the flange t2, not the depth H.
Does JIS G 3101 specify an impact test for SS400?
No. There is no Charpy requirement for SS400 in JIS G 3101. A toughness value must not be inferred from the grade name. If a defined impact test is required, nominate a standard and quality that actually table it, such as a JIS G 3106 grade.
Are C, Si and Mn limited in SS400?
JIS G 3101:2024 Table 2 gives phosphorus and sulphur maxima of 0.050% for SS400. Carbon and manganese are shown as dashes, not as numerical maxima, and silicon is not a tabulated column for this grade. Elements shown as dashes, and elements not listed, may be added as necessary and shall be reported if they are.
Why does this page list both t1 and t2 in the designation?
The standard allows thickness to be displayed as t1 only, but several depths share the same H and B with different web and flange thicknesses — for example the two 150×75 rows and the three 380×100 rows. The full H×B×t1×t2 designation avoids mixing those sections.
Which standards should appear on the inspection document?
At least JIS G 3101 and its edition, the grade SS400, the JIS G 3192 designation, the delivery condition, heat analysis including any added elements, and tensile results by thickness. If not otherwise specified, the inspection document is a JIS G 0415 inspection certificate 3.1.

Request a Quotation for JIS G 3101 SS400 Steel Channel

JIS G 3101 SS400 steel channel is a general-structure section with a 400–510 N/mm² tensile range and 245 N/mm² minimum yield up to 16 mm. Nominate the JIS G 3192 channel size (H×B×t1×t2) and the material to JIS G 3101:2024 (or the edition on the order). The table is the standard Table 12 series, used as reference dimensions, not a rolling list. Send the size list, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X