GOST 19281 10KhSND Steel Plate | 10KhSND HSLA Rolled Steel Plate | GOST 19281 Steel - SHH STEEL

GOST 19281 10KhSND Steel Plate | 10KhSND HSLA Rolled Steel Plate

GOST 19281 10KhSND (10ХСНД) steel plate is a chromium-silicon-nickel-copper high-strength rolled steel under GOST 19281-2014, whose official English title is High strength rolled steel. General specification. The ordering property is the strength class, not the grade name alone. The letter D in the designation is part of the base grade: clause 5.2.1.3 provides for increased resistance to atmospheric corrosion, guaranteed by the chemical composition and the manufacturing technology. Annex A Table A.2 lists this grade for plate, universal wide strip and bent profiles in class 375 up to 10 mm (Amendment 1 replaced that row — 10KhSND remains listed; confirm official companions) and in class 390 up to 50 mm. Table 7 lists 10KhSND under alloyed steels, with carbon not more than 0.12 %, silicon 0.80–1.10 %, manganese 0.50–0.80 %, chromium 0.60–0.90 %, nickel 0.50–0.80 % and copper 0.40–0.60 %. This page is written to the 2014 edition, with Amendment 1 where that amendment is known, and does not tabulate 2025 requirements.
Grade
10KhSND
Standard
GOST 19281-2014
Official English title
High strength rolled steel. General specification.
Table A.2 plate classes
375 (≤10 mm, Amd 1 — confirm companions); 390 (≤50 mm)
Table 7 C / Si / Cr-Ni-Cu
C ≤0.12 %; Si 0.80–1.10 %; Cr 0.60–0.90 %; Ni 0.50–0.80 %; Cu 0.40–0.60 %
Table 10 at class 390 (2016)
ReH 390 N/mm²; Rm 510 N/mm²; A 19 %
CEV, GS option (Amd 1)
0.51 % permitted at 345/375/390 without Ti+B; Pcm ≤0.30 % with Ti+B
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

General Description of GOST 19281 10KhSND Steel Plate

GOST 19281 10KhSND Steel Plate is listed in Table 7 under alloyed steels. Among the 10KhSND, 15KhSND and 10KhNDP group it has the highest silicon (0.80–1.10 %), the highest nickel (0.50–0.80 %) and the highest copper (0.40–0.60 %), with carbon not more than 0.12 % and chromium 0.60–0.90 %, the same chromium range as 15KhSND. Phosphorus is a maximum of 0.030 %, not the 0.070–0.120 % range of 10KhNDP. Table A.2 places 10KhSND at classes 375 and 390, whereas 15KhSND and 10KhNDP are recommended at class 345 only. A shared reputation as atmospheric-corrosion-resistant steel is not interchangeability. Amendment 1 note 4 requires aluminium deoxidation of 0.02–0.06 % for 10KhSND, and Amendment 1 note 9 permits optional titanium-boron microalloying by agreement.

Table 7 has no 10KhSND-1 composition-1 row; this page does not invent one. The letter D is already in the base designation and is not a separate suffix article. Related weathering-resistant structural steel under ISO 630-5 is a different system, not a substitute for a GOST 19281 order.

GOST 19281 10KhSND Steel Plate Material Specification

As of 12 November 2026, GOST 19281-2014 remains in force. It was introduced on 1 January 2015, replaces GOST 19281-89, and has restricted validity until 1 December 2026. It is applied with Amendment 1, which has been in force from 1 June 2020. This page is written to the 2014 edition, with Amendment 1 where that amendment is known. GOST 19281-2025 has been adopted and takes effect on 1 December 2026, so buyers should confirm which edition applies to their order. The 2025 edition has a right of early application; this page does not tabulate 2025 requirements. Two one-page corrections issued after Amendment 1 were not inspected for this page; confirm any later correction against the official text of the edition stated on the order.

The official English title of GOST 19281-2014 is “High strength rolled steel. General specification.” The standard covers hot-rolled plate, universal wide strip, bars, sections and bent profiles of high strength for general-purpose structures with welded, riveted or bolted connections. This page is the plate product. Table A.2 recommends 10KhSND at class 375 up to 10 mm (Amendment 1 replaced that row; 10KhSND remains listed — confirm official companions) and at class 390 up to 50 mm (a dedicated row up to 40 mm, and a row up to 50 mm with the 14G2AF family). It does not list 10KhSND at class 345.

Order the plate by strength class and by grade. The classes used in the standard are 265, 295, 315, 325, 345, 355, 375, 390 and 440. Each class is a specified minimum yield strength in N/mm², subject to any higher Table 10 cell for a named grade and thickness. Inspection categories, delivery condition, guaranteed weldability (GS) and any listed variant must be stated on the order; they are not implied by the grade name.

GOST 19281 10KhSND Steel Plate Chemical Composition

The ladle analysis below was read from Table 7 of the 2016 reprint (alloyed-steels heading, PDF page 19). Amendment 1 does not change these numeric cells. Values are mass fraction, in %.

Grade C Si Mn P S max Cr Ni Cu V Other
10KhSND ≤0.12 0.80–1.10 0.50–0.80 0.030 max 0.035 0.60–0.90 0.50–0.80 0.40–0.60 ≤0.12 —

Table 7 is ladle analysis, read from the 2016 reprint under the alloyed-steels heading. Amendment 1 does not change the numeric chemistry cells for 10KhSND, 15KhSND or 10KhNDP. Table 8 gives product-analysis deviations, also read from the 2016 reprint, with the Amendment 1 boron row noted below where it applies. For elements whose Table 7 cell is an upper limit only, Table 8 note 2 applies only the plus deviations. Carbon on 10KhSND and 10KhNDP is an upper limit only (not more than 0.12 %), so only the plus carbon deviation applies in the product analysis of those grades. Carbon on 15KhSND is a range, so both the plus and the minus carbon deviations apply.

Element Product-analysis deviation, %
C ±0.02
Mn ±0.10
Si ±0.05
Cr ±0.05
Ni ±0.05
Cu ±0.05
S ±0.005
P +0.005 (plus only)
N ±0.005
V +0.02 / −0.01
Ti +0.010 / −0.005
Nb +0.010 / −0.005
Al +0.010 / −0.005

Arsenic shall not exceed 0.08 % in steel of all grades (Table 7 note 1). Nitrogen in steel that is not alloyed with nitrogen shall not exceed 0.008 % without secondary metallurgy, or 0.010 % with secondary metallurgy. Amendment 1 allows nitrogen up to 0.012 % inclusive provided the product meets the official Tables 11 and 12 for impact after mechanical ageing, regardless of the ordered category, including an order without a category. A further nitrogen-equivalent provision is stated in note 3; confirm that provision against the official text. These three grades have no specified nitrogen-alloying range in Table 7.

Amendment 1, Table 7 note 4, requires aluminium deoxidation of 0.02–0.06 % for grades 09G2, 09G2-1, 09G2S, 09G2S-1 and 10KhSND. That requirement applies to 10KhSND. The actual aluminium mass fraction, controlled in the ladle sample, is stated in the quality document. It does not apply to 15KhSND or 10KhNDP from this note. Amendment 1 note 5 still permits additional microalloying with aluminium, titanium and niobium, calculated to give aluminium not more than 0.05 %, titanium not more than 0.04 % and niobium not more than 0.05 %, unless other mass fractions are stated in Table 7; those elements are controlled and stated in the quality document when that option is used.

Amendment 1, Table 7 note 9: by agreement between the manufacturer and the purchaser, 10KhSND may be microalloyed with titanium and boron together, calculated to give titanium not more than 0.04 % and boron not more than 0.005 %. That option is not implied by the grade name; state it on the order if it is required. Amendment 1 also adds a Table 8 product-analysis deviation for boron of +0.0005 % on 10KhSND so microalloyed. Annex B of the amendment records a further optional 10KhSND product with molybdenum not more than 0.08 %; that is an agreed option, not a mandatory Table 7 cell. Confirm the official annex if that option is ordered. Amendment 1 note 11 names only 09G2S and 17G1S and does not apply to 10KhSND. Table 7 note 8 does not name 10KhSND.

Clause 5.2.1.3 provides that, when the steel designation includes the letter D, the product is supplied with increased resistance to atmospheric corrosion, guaranteed by the chemical composition and the manufacturing technology. That letter is part of the base designations 10KhSND, 15KhSND and 10KhNDP; it is not a separate suffix variant on these pages. This is not a tabulated corrosion rate, not a coating specification, and not a formal weathering-grade equivalence. Confirm the official clause. Related weathering-resistant structural steel is published under ISO 630-5; that system is not equivalent to GOST 19281 and is not a substitute without engineer review of both complete specifications.

GOST 19281 10KhSND Steel Plate Mechanical Properties

Annex A is a recommended annex. Table A.2 lists grades that provide the stated strength class at the stated thickness for plate, universal wide strip and bent profiles. A listing in Table A.2 is not a certificate that every thickness in the band is interchangeable with every other grade in the same cell, and it is not a substitute for the Table 10 tensile minima of the ordered class. Footnote * permits controlled rolling (KP) or controlled rolling followed by accelerated cooling. Footnote ** permits controlled rolling, thermomechanical treatment (TMO) or thermal strengthening (TY). Amendment 1 replaced only the class 375 row of Table A.2; the other rows below were visually read from the 2016 reprint, which Amendment 1 does not rewrite.

For 10KhSND, Table A.2 lists the following recommended plate combinations:

Strength class Thickness in Table A.2 10KhSND listed Table A.2 footnote Source of the row
375 Up to 10.0 mm inclusive 10KhSND, with the 10G2B and 15GF families in the 2016 row — confirm official Amendment 1 companions — on the 10KhSND name Amendment 1 replaced this class-375 row. 10KhSND remains listed in the up-to-10 mm band. Confirm the official companion designations. This page does not publish “09G2S-G”, and does not present the 2016 companion list as the current official list.
390 Up to 40.0 mm inclusive (dedicated row); and up to 50.0 mm inclusive with the 14G2AF family 10KhSND in both of those 390 rows — 2016 visual; Amendment 1 does not rewrite this class. Table A.2 therefore recommends 10KhSND at class 390 up to 50 mm.

Table 10 gives minimum yield strength (ReH, σ_T), tensile strength (Rm, σ_B) and percentage elongation after fracture (δ5) for plate, universal wide strip and bent profiles. The yield minimum equals the strength class, except where Table 10 states a higher figure for a named grade group. Amendment 1 rewrote the thickness column of Table 10 for strength classes 295, 345, 355 and 440. The yield, tensile-strength and elongation minima below were read from the 2016 reprint of Table 10, whose mechanical columns Amendment 1 did not describe as replaced. Use the official Amendment 1 (2021 consolidated) table for the current thickness bands of those four classes, including any footnote that applies to thicker product. A 2016 footnote that treated some thicker bands as non-rejectable until 1 January 2016 has elapsed.

Table 10 lists 10KhSND at class 375 up to 50 mm with ReH 375 N/mm², Rm 510 N/mm² and elongation 20 %, and at class 390 up to 50 mm with ReH 390 N/mm², Rm 510 N/mm² and elongation 19 %. Table A.2 recommends class 375 only up to 10 mm; above 10 mm the Table 10 class 375 listing is not an A.2 recommendation. 10KhSND is not in the Table 10 groups for class 345 as read from the 2016 reprint.

Strength class Thickness label in the 2016 Table 10 (see the Amendment 1 note) ReH min, N/mm² Rm min, N/mm² Elongation δ5 min, % Grade group and A.2 relationship
375 Up to 50.0 mm inclusive (thickness column not amended) 375 510 20 10KhSND with 09G2S, 14G2AF, 17G1S, 15GF and 10G2B. Table A.2 recommends 10KhSND at class 375 only up to 10 mm; above 10 mm this is a Table 10 listing, not an A.2 recommendation.
390 Up to 50.0 mm inclusive (not amended) 390 510 19 10KhSND with 10G2S1, 14G2, 14G2AF, 16G2AF and other named grades. Aligns in span with the Table A.2 recommendation up to 50 mm. A shared Table 10 cell is not interchangeability.

Impact toughness for plate is specified in Table 12, which Amendment 1 replaced in full, and is selected by the inspection category ordered from Table 4, which Amendment 1 also replaced. Values are minima in J/cm² for KCU or KCV at the temperatures listed for that category, class, grade and thickness. A plus sign in Table 12 means the test is made to collect statistical data; the result is recorded in the quality document and is not a specified minimum. A minus sign means the property is not specified and is not tested. This page does not tabulate Table 12 cells, because an official-format 2021 (Amendment 1) Table 12 was not visually inspected and a third-party extract is not a substitute for that inspection. If impact is required, state the category, the temperature and the test type on the order, and confirm the current figures against the official table of GOST 19281-2014 with Amendment 1.

Amendment 1 marked some Table 12 cells as optional for two years from 1 June 2020. That two-year period has elapsed. Confirm the current application of those footnote cells, and of any later one-page correction, against the official text. Do not take impact figures from the 2016 reprint, from another standard, or from a handbook and apply them as the current official minima.

Amendment 1 deletes clause 5.2.1.6, which in the 2016 reprint required a 180° bend on a mandrel of diameter equal to two specimen thicknesses and allowed the manufacturer to omit the test if it guaranteed satisfactory results at the purchaser. That deleted clause is not restated on this page as a current requirement. The amended acceptance rules still provide for recording a 180° bend result, or a manufacturer’s guarantee of that bend, on the quality document. Confirm the current bend requirement against the official 2014 text with Amendment 1.

Table 10 may list a grade in a thickness band that Table A.2 does not recommend. A Table 10 listing is the tensile requirement if that class and thickness are ordered; it is not, by itself, a Table A.2 recommendation. State the class on the order.

GOST 19281 10KhSND Steel Plate Delivery Conditions

The strength class is the ordering property. State the edition that applies to the order (see the Material Specification), the grade (including any composition-1 or copper-bearing D variant listed on this page), the strength class, the inspection category, the dimensions, the quantity and the delivery condition. Table A.2 recommends 10KhSND plate at class 375 up to 10 mm (Amendment 1 row — confirm official companions) and at class 390 up to 50 mm. A Table A.2 listing is a recommended combination of grade, class and thickness; it is not a substitute for stating the class on the order, and it is not interchangeability with other grades listed in the same cell.

Delivery may be agreed as hot-rolled, heat-treated, or with controlled rolling (KP), controlled rolling followed by accelerated cooling, thermomechanical treatment (TMO) or thermal strengthening (TY), where Table A.2 or the order permits those routes (footnotes * and ** in Table A.2). Do not assume a heat-treated or thermomechanically treated delivery from the grade name alone. Record the actual condition on the quality document. If the purchaser will heat-treat the article after delivery, see Table 7 note 7 before selecting a composition-1 variant.

Table 7 has no 10KhSND-1 row. This page does not invent a composition-1 variant. The letter D is part of the base designation. Optional (Ti+B) microalloying, and the optional molybdenum-limited product recorded in the amendment’s Annex B, are order agreements, not separate articles; state them on the order if they are required.

Clause 5.2.1.3 provides that, when the steel designation includes the letter D, the product is supplied with increased resistance to atmospheric corrosion, guaranteed by the chemical composition and the manufacturing technology. That letter is part of the base designations 10KhSND, 15KhSND and 10KhNDP; it is not a separate suffix variant on these pages. This is not a tabulated corrosion rate, not a coating specification, and not a formal weathering-grade equivalence. Confirm the official clause. Related weathering-resistant structural steel is published under ISO 630-5; that system is not equivalent to GOST 19281 and is not a substitute without engineer review of both complete specifications.

GOST 19281 10KhSND Steel Plate Weldability

When guaranteed weldability (designated GS) is ordered, Amendment 1 to clause 5.2.1.2 limits the carbon equivalent CEV to not more than 0.43 % for strength classes 265, 295, 315 and 325; 0.46 % for classes 345, 355 and 375; 0.48 % for class 390; and 0.51 % for class 440. The same clause also requires the manufacturing technology and the chemical composition, including the Table 8 product-analysis deviations, to support weldability. GS is not implied by the grade name; state it on the order if it is required.

For 10KhSND, Amendment 1 to clause 5.2.1.2 adds two provisions that differ from the general CEV limits above. When 10KhSND is ordered without titanium-boron microalloying, carbon equivalent not more than 0.51 % is permitted for strength classes 345, 375 and 390 (the general limits at those classes are 0.46 % and, at 390, 0.48 %). When 10KhSND is ordered with (Ti+B) microalloying, weldability is ensured by a cracking parameter Pcm of not more than 0.30 %. The amendment provided for that Pcm figure to be refined after two years of statistical data from 1 June 2020; that two-year period has elapsed. Confirm the current application of the Pcm limit, and the official calculation at clause 7.2.1, against the official 2014 text with Amendment 1. This page does not tabulate the Pcm formula. State (Ti+B) on the order if that route is required; it is not implied by the grade name. Guaranteed weldability (GS) is itself an ordered option.

This page does not give preheat, interpass, heat-input or post-weld heat-treatment figures. The fabricator is responsible for welding-procedure qualification, consumable selection, preheat and any post-weld heat treatment required by the project specification. Do not take those figures from another standard or from a handbook and apply them as GOST 19281 rules. A shared strength class, a Table A.2 listing alongside another grade, or a commonly compared foreign designation does not make those grades automatic welding substitutes. A related weathering-resistant designation is not a welding substitute either.

GOST 19281 10KhSND Steel Plate Tolerances

Dimensions, shape and permissible deviations for plate follow the plate-dimension standard cited by GOST 19281-2014 as updated by Amendment 1. State the required thickness, width, length, thickness-accuracy class, edge condition and, for plate supplied as sheets, the flatness class on the order. This page does not tabulate numerical deviation limits from that dimension standard.

Surface quality and dressing limits are those of GOST 19281-2014 with Amendment 1. Confirm the permitted defect types, dressing depth and area, and the prohibition on delamination against the official text. Ultrasonic testing is not a default requirement. If continuity testing is required, state the method, the class and the test volume on the order; they are not implied by the grade or the strength class.

GOST 19281 10KhSND Steel Plate Applications and service limits

10KhSND under GOST 19281-2014 is general-purpose high-strength rolled steel for welded, riveted or bolted structures. Typical uses are structural members, frames and fabricated platework where the ordered strength class, thickness and inspection category match the design. This page does not assign a design stress, a temperature limit or a code approval. Those come from the project specification and the design standard, not from the grade name.

Table A.2 does not recommend 10KhSND at class 345, and recommends class 375 only up to 10 mm. Table 10 lists class 375 up to 50 mm; above 10 mm that listing is not an A.2 recommendation. The atmospheric-corrosion provision is not a tabulated corrosion rate and is not a substitute for a project coating or a formal weathering specification. Related ISO 630-5, EN 10025-5 or GB/T 4171 designations are not approved substitutes without engineer review. Do not use this plate as a boiler or pressure-vessel product solely because the same designation appears under GOST 5520; that is a different product standard with its own thickness, category and test regime. Do not treat a commonly compared foreign structural grade as approved for the same duty without engineer review of both complete specifications.

Compare 10KhSND with related GOST 19281 grades

These three GOST 19281 grades are chromium-nickel-copper alloyed steels. The letter D in each base designation marks the copper-bearing, atmospheric-corrosion provision of clause 5.2.1.3. They differ in carbon, silicon, phosphorus, the chromium-nickel-copper ranges, the Table A.2 class listings, and selected Table 10 cells. 10KhNDP is the phosphorus-bearing grade (the letter P). They are related, not equivalent. A shared strength class or a shared reputation as atmospheric-corrosion-resistant steel is not interchangeability. Sister GOST 19281 product pages are not linked here because those URLs are not live; the designations are named for comparison only.

Grade Table 7 distinctive chemistry Table A.2 plate classes (summary) Distinctive Table 10 cell
10KhSND (this plate) C ≤0.12; Si 0.80–1.10; Mn 0.50–0.80; Cr 0.60–0.90; Ni 0.50–0.80; Cu 0.40–0.60; P 0.030 max. Note 4 Al 0.02–0.06 % mandatory. Optional (Ti+B). 375 (≤10 mm, Amd 1 — confirm companions); 390 (≤40 mm dedicated; also ≤50 mm with 14G2AF) Class 375: 375 / 510 / 20 % (T10 up to 50 mm; A.2 only ≤10 mm). Class 390: 390 / 510 / 19 %.
15KhSND C 0.12–0.18; Si 0.40–0.70; Mn 0.40–0.70; Cr 0.60–0.90; Ni 0.30–0.60; Cu 0.20–0.40; P 0.030 max. Note 4 Al does not apply. 345 (≤50 mm, second sub-row) Class 345: 345 / 490 / 21 % (confirm official Amd 1 thickness). Not the 10KhNDP 470 / 20 % cell.
10KhNDP C ≤0.12; Si 0.17–0.37; Mn 0.30–0.60; P 0.070–0.120; Cr 0.50–0.80; Ni 0.30–0.60; Cu 0.30–0.50; Al 0.08–0.15. Table 8 note 1 for P and Al. 345 (≤50 mm, first sub-row) Class 345: 345 / 470 / 20 % — dedicated cell, lower Rm and elongation than 15KhSND at the same class.

GOST 19281 10KhSND Steel Plate Equivalent Material Grade

No formal equivalence has been verified for the designations below. They are related designations only and are not equivalent to this GOST 19281-2014 plate. Official correspondence or equivalent-grade tables were not inspected for this page; confirm any claimed equivalent against the official texts of both standards and the project specification. Engineer approval is required before any substitution. This page does not link any external catalogue. None of those relationships is interchangeability.

Standard Country-Region Equivalent Grade Note
GOST 19281-2014 Interstate (GOST) 10KhSND This page’s designation. Not an equivalent of another grade.
ISO 630-5 International (ISO) — (family; no grade assigned on this page) Related weathering-resistant structural steel family. Not equivalent. Official correspondence tables were not inspected. Verify chemistry, strength class, thickness, delivery, toughness and the project specification. Engineer approval is required. Not a verified formal equivalent.
EN 10025-5 Europe — (family; no grade assigned on this page) Related weathering-resistant structural plate family. Not equivalent. This page does not assign a lettered EN grade as a formal equivalent. Engineer approval is required. Not a verified formal equivalent.
GB/T 4171 China — (family; no grade assigned on this page) Related atmospheric-corrosion-resistant structural plate family. Not equivalent. This page does not assign a Q355NH-class designation as a formal equivalent. Engineer approval is required. Not a verified formal equivalent.

Related weathering-resistant structural plate systems include ISO 630-5, EN 10025-5 and GB/T 4171. Related high-strength structural plate systems, including GB/T 1591, EN 10025-2 and ASTM A572, are sometimes listed on comparison charts as well. No grade in those systems is listed as a verified equivalent on this page. A chart cannot replace a review of chemistry, including chromium, nickel, copper and (for 10KhNDP) phosphorus, strength class, product form, delivery condition, mechanical tests and the project specification. A similar yield class, or a shared reputation as atmospheric-corrosion-resistant steel, does not authorise substitution.

Why choose Us

SHH STEEL produces and exports GOST 19281 plate, including GOST 19281 10KhSND Steel Plate. We review the ordered strength class (375 or 390 as agreed), the ladle analysis against Table 7, including the 0.02–0.06 % aluminium deoxidation and any agreed (Ti+B) option, and the Table 10 tensile minima before production, and we state the actual results on the quality document. We do not treat a shared strength class, a Table A.2 cell shared with another grade, or a commonly compared foreign designation as a substitute for the ordered grade and class.

Orders are accepted against GOST 19281-2014, including Amendment 1, unless the order states the 2025 edition. Enquiry details should include the edition, grade (and any listed variant), strength class, inspection category, thickness, width, length, quantity, delivery condition and any agreed options (guaranteed weldability GS, ultrasonic class, microalloying agreement). See the GOST 19281 hub for the product family.

Our Service

Supply covers production to the ordered 2014 requirements, including Amendment 1, or to the 2025 edition if that is the edition stated on the order, together with mill documentation and export packing and shipment. Quality documents record the actual ladle analysis, tensile results for the ordered class, and, where the category requires them, impact results, including any characteristic that Table 12 marks as determined for statistical data. Guaranteed weldability and ultrasonic testing are supplied when they are agreed on the order, not by default.

To enquire, state the edition (GOST 19281-2014 with Amendment 1, or GOST 19281-2025 if that edition applies), grade 10KhSND, the strength class, the inspection category, dimensions, quantity and the required options. SHH STEEL will confirm manufacturability and the inspection plan against that order. This page is a product description written to the 2014 edition with Amendment 1; the official standard of the edition on the order, and the quality document, govern acceptance.

FAQ

What is 10KhSND steel plate?

10KhSND steel plate is a chromium-silicon-nickel-copper high-strength rolled steel under GOST 19281-2014. Table 7 lists it under alloyed steels, with carbon not more than 0.12 %, silicon 0.80–1.10 %, manganese 0.50–0.80 %, chromium 0.60–0.90 %, nickel 0.50–0.80 % and copper 0.40–0.60 %. The letter D is part of the base designation; clause 5.2.1.3 provides for increased resistance to atmospheric corrosion, guaranteed by chemistry and manufacturing technology. The ordering property is the strength class. Table A.2 recommends it at class 375 up to 10 mm (Amendment 1 — confirm official companions) and at class 390 up to 50 mm.

Is GOST 19281-2014 still current for 10KhSND?

Yes, as of 12 November 2026. GOST 19281-2014 remains in force, applied with Amendment 1 from 1 June 2020, and has restricted validity until 1 December 2026. This page is written to the 2014 edition, with Amendment 1 where that amendment is known. GOST 19281-2025 has been adopted and takes effect on 1 December 2026, so buyers should confirm which edition applies to their order. The 2025 edition has a right of early application. State the edition, and Amendment 1 if the 2014 edition is ordered, together with the grade and the strength class, on the order. This page does not tabulate 2025 tables. Two one-page corrections issued after Amendment 1 were not inspected for this page.

Which strength classes can 10KhSND plate be ordered in?

Table A.2 recommends 10KhSND at class 375 up to 10 mm (Amendment 1 replaced that row; 10KhSND remains listed — confirm official companions) and at class 390 up to 50 mm. It does not list 10KhSND at class 345. Table 10 gives 375 / 510 / 20 % at class 375 up to 50 mm (the portion above 10 mm is not an A.2 recommendation) and 390 / 510 / 19 % at class 390 up to 50 mm. Those two Table 10 classes were not in the Amendment 1 thickness rewrite. State the class on the order.

How does 10KhSND differ from 15KhSND and from 10KhNDP?

Against 15KhSND: 10KhSND has lower carbon (not more than 0.12 % against 0.12–0.18 %), higher silicon (0.80–1.10 % against 0.40–0.70 %), higher nickel (0.50–0.80 % against 0.30–0.60 %) and higher copper (0.40–0.60 % against 0.20–0.40 %), with the same chromium range (0.60–0.90 %). Table A.2 places 10KhSND at 375 and 390, and 15KhSND at 345 only. Against 10KhNDP: 10KhSND has much higher silicon, higher chromium, nickel and copper, and phosphorus as a 0.030 % maximum, not a 0.070–0.120 % range. Table 10 at class 345 gives 10KhNDP a dedicated 345 / 470 / 20 % cell; 10KhSND is not in that class-345 group. Note 4 aluminium deoxidation and the (Ti+B) option apply to 10KhSND, not to the other two from those notes. A shared atmospheric-corrosion letter D is not interchangeability.

Does 10KhSND need special aluminium deoxidation or titanium-boron microalloying?

Aluminium deoxidation of 0.02–0.06 % is a mandatory Table 7 note 4 requirement for 10KhSND (Amendment 1); the actual ladle aluminium is stated in the quality document. Titanium-boron microalloying is optional, by agreement, under Amendment 1 note 9 (titanium not more than 0.04 %, boron not more than 0.005 %). It is not implied by the grade name. When (Ti+B) is used and guaranteed weldability is ordered, Amendment 1 limits Pcm to not more than 0.30 %. Without (Ti+B), at classes 345, 375 and 390, CEV not more than 0.51 % is permitted. Confirm the official amendment, including current application of the Pcm figure. Table 7 has no 10KhSND-1 row; this page does not invent one.

Enquire about GOST 19281 10KhSND Steel Plate

Enquire for GOST 19281 10KhSND Steel Plate to GOST 19281-2014, including Amendment 1, or to GOST 19281-2025 if that is the edition that applies to the order. State the grade 10KhSND, the strength class, the inspection category, dimensions, quantity, the delivery condition and any agreed options. SHH STEEL will confirm the inspection plan against the official tables of the edition on the order. The official standard and the quality document govern acceptance.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X