GB/T 706 Q355B Steel Channel

GB/T 706 Q355B steel channel is a taper-flange Chinese channel in as-rolled low-alloy steel Q355B (GB/T 1591-2018), with 355 MPa minimum yield up to 16 mm and 34 J longitudinal impact at +20 °C. Sizes use GB/T 706-2016 as the numeric basis. The ordered edition governs. SHH STEEL reviews grade, condition, designation and certificate requirements before quoting.
Keywords
GB/T 706 Q355B Steel Channel, Q355B channel, as-rolled Q355B channel, GB/T 706 channel, Chinese steel channel
Equivalent Grades:
Near-equivalents only, not automatic substitutes: former Q345B; Q355C/D; S355JR; ASTM A572 Grade 50.
Share:
General Description
Material Specification
Available Sizes of Q355B Steel Channel
Chemical Composition
Carbon Equivalent
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why Source Q355B Steel Channels from SHH STEEL
FAQ
Conclusion

What is GB/T 706 Q355B Steel Channel?

GB/T 706 Q355B steel channel is a hot-rolled Chinese taper-flange channel whose material grade is as-rolled Q355B under GB/T 1591 and whose shape, tolerances and theoretical mass are ordered to GB/T 706. Q stands for yield strength, 355 is the minimum upper yield strength in MPa for the thinnest tabulated thickness band, and B is the quality grade. For quality B the Charpy V-notch requirement is 34 J on a longitudinal specimen, or 27 J on a transverse specimen, at +20 °C. Longitudinal specimens are the default; transverse testing is by agreement.

This page covers the rolled channel, not plate and not an H-section. The same grade in plate form is listed separately as Q355B steel plate (GB/T 1591). Sampling direction, elongation and some thickness-band footnotes differ between plates and sections, so the plate page is not a substitute data sheet for channels, and neither is GB/T 11263 Q355B H-beam. GB/T 1591 itself refers the dimensions, shape, mass and tolerances of hot-rolled section steel to GB/T 706.

These bars are filed under steel channel profiles in the steel structural profiles category. They are Chinese taper-flange channels (the inner face of the flange is sloped). They are not European UPN or UPE, American C or MC, or Japanese channels of a similar millimetre depth, and they are not GB/T 11263 H-sections or GB/T 706 I-beams. A Q355B angle to GB/T 706 is a different product, with its own designation and its own page when that page is published.

Q355B is the current as-rolled 355 MPa quality-B grade in GB/T 1591-2018, which replaced the former Q345 designation. It is a high-strength low-alloy structural steel for building frames, plant structures and general fabrication where a +20 °C impact quality is accepted. It is not Q355N or Q355M, not a weathering grade, and not a pressure-vessel or nuclear safety material. An enquiry that still says only “Q345B channel” should be confirmed against the 2018 designation, the as-rolled condition and the dimensional standard before rolling.

Material, Dimensions and Tolerances for Q355B Channels

Three documents should appear, separately, on the purchase order and on the inspection certificate:

  • GB/T 1591 is the material standard for high-strength low-alloy structural steels. This article uses the as-rolled Q355B chemistry, carbon equivalent, tensile and impact values published in GB/T 1591-2018. Normalized (N) and thermomechanical (M) Q355 grades have their own tables and are a different order. The edition named on the order governs acceptance.
  • GB/T 706 is the product standard for hot-rolled section steel, including these taper-flange channels. It sets the size series, dimensional and shape tolerances, theoretical mass and section surface rules, and it points chemistry and mechanical properties to GB/T 700 or GB/T 1591. It is not itself the material certificate. The size table below is the complete standard channel series in GB/T 706-2016 Table A.2. GB/T 706-2016 is used as the numeric basis. GB/T 706-2026 is the successor edition, with implementation from 1 December 2026. The edition of GB/T 706 named on the order governs dimensional acceptance.
  • Tolerances on depth, flange width, web and flange thickness, out-of-square, length, straightness and mass are those of the ordered GB/T 706 edition, not of GB/T 1591 and not of GB/T 11263.

A mill may certify Q355B on a European or Japanese channel, or roll a Chinese channel to a different material standard, if that combination is in its programme and is fully documented. Matching a nominal 200 mm or 8 in depth is not a substitution.

Q355B Channel Sizes: GB/T 706 Standard Channel Series

The table lists the complete standard channel series in GB/T 706-2016 Table A.2: 41 sizes, from model 5 (50×37×4.5) to model 40c (400×104×14.5). The usual designation is the model number, with a letter where the standard distinguishes a, b or c flanges at the same depth — for example 16a, 16b, 20a, 20b or 40c — or the depth × flange × web string such as [200×75×9, often abbreviated [20b. Theoretical mass uses a density of 7.85 g/cm³. The root radii in GB/T 706 are for roll-pass design and are not delivery conditions, so they are not listed in the size table. Use the table to identify and estimate, not as a rolling programme for Q355B. Mid-range models such as 10, 16a and 20b are the usual enquiry core; the 5 and 6.3 rows and the 36 and 40 rows should be confirmed size by size.

GB/T 706-2016 is used as the numeric basis. GB/T 706-2026 is the successor edition, with implementation from 1 December 2026. The edition of GB/T 706 named on the order governs dimensional acceptance. This page does not invent rows that Table A.2 does not list, and it does not treat a Chinese 20b as interchangeable with a European UPN 200 or an American C8 of similar depth.

Because GB/T 706 directs channel specimens taken under GB/T 2975 to the web, the thickness band is ordinarily the web thickness d. All tabulated standard channels have a web of 14.5 mm or less, so they remain in the first (355 MPa / 22% / CEV 0.45) bands when the web is the test location. Do not apply the flange thickness t as if it were the sampled thickness unless the order relocates the specimen.

Swipe horizontally to view all dimensions.

Model Designation (h×b×d) h (mm) b (mm) d (mm) t (mm) A (cm²) Mass (kg/m)
5 50×37×4.5 50 37 4.5 7.0 6.925 5.44
6.3 63×40×4.8 63 40 4.8 7.5 8.446 6.63
6.5 65×40×4.3 65 40 4.3 7.5 8.292 6.51
8 80×43×5.0 80 43 5.0 8.0 10.24 8.04
10 100×48×5.3 100 48 5.3 8.5 12.74 10.0
12 120×53×5.5 120 53 5.5 9.0 15.36 12.1
12.6 126×53×5.5 126 53 5.5 9.0 15.69 12.3
14a 140×58×6.0 140 58 6.0 9.5 18.51 14.5
14b 140×60×8.0 140 60 8.0 9.5 21.31 16.7
16a 160×63×6.5 160 63 6.5 10.0 21.95 17.2
16b 160×65×8.5 160 65 8.5 10.0 25.15 19.8
18a 180×68×7.0 180 68 7.0 10.5 25.69 20.2
18b 180×70×9.0 180 70 9.0 10.5 29.29 23.0
20a 200×73×7.0 200 73 7.0 11.0 28.83 22.6
20b 200×75×9.0 200 75 9.0 11.0 32.83 25.8
22a 220×77×7.0 220 77 7.0 11.5 31.83 25.0
22b 220×79×9.0 220 79 9.0 11.5 36.23 28.5
24a 240×78×7.0 240 78 7.0 12.0 34.21 26.9
24b 240×80×9.0 240 80 9.0 12.0 39.01 30.6
24c 240×82×11.0 240 82 11.0 12.0 43.81 34.4
25a 250×78×7.0 250 78 7.0 12.0 34.91 27.4
25b 250×80×9.0 250 80 9.0 12.0 39.91 31.3
25c 250×82×11.0 250 82 11.0 12.0 44.91 35.3
27a 270×82×7.5 270 82 7.5 12.5 39.27 30.8
27b 270×84×9.5 270 84 9.5 12.5 44.67 35.1
27c 270×86×11.5 270 86 11.5 12.5 50.07 39.3
28a 280×82×7.5 280 82 7.5 12.5 40.02 31.4
28b 280×84×9.5 280 84 9.5 12.5 45.62 35.8
28c 280×86×11.5 280 86 11.5 12.5 51.22 40.2
30a 300×85×7.5 300 85 7.5 13.5 43.89 34.5
30b 300×87×9.5 300 87 9.5 13.5 49.89 39.2
30c 300×89×11.5 300 89 11.5 13.5 55.89 43.9
32a 320×88×8.0 320 88 8.0 14.0 48.50 38.1
32b 320×90×10.0 320 90 10.0 14.0 54.90 43.1
32c 320×92×12.0 320 92 12.0 14.0 61.30 48.1
36a 360×96×9.0 360 96 9.0 16.0 60.89 47.8
36b 360×98×11.0 360 98 11.0 16.0 68.09 53.5
36c 360×100×13.0 360 100 13.0 16.0 75.29 59.1
40a 400×100×10.5 400 100 10.5 18.0 75.04 58.9
40b 400×102×12.5 400 102 12.5 18.0 83.04 65.2
40c 400×104×14.5 400 104 14.5 18.0 91.04 71.5

Q355B Chemical Composition for Channels (GB/T 1591 As-Rolled Ladle Analysis)

The figures below are ladle-analysis maxima for as-rolled Q355B in GB/T 1591-2018 Table 1. They are limits, not typical heat results. Product analysis, when required, follows the deviations in GB/T 222. These values are not the Table 3 or Table 5 limits used for Q355N or Q355M, and they should not be taken from unofficial trader sheets that still quote a 0.20% carbon cap or a 0.030% phosphorus cap as if those were the quality-B as-rolled defaults. Quality C and D of the same steel grade use a thickness-split carbon table and tighter phosphorus and sulphur; those are different quality letters, not a silent tightening of Q355B. The certificate still has to identify the channel, not a plate or H-beam heat that happens to share the name.

Element Maximum, ladle analysis (mass %) Notes for as-rolled Q355B channels
C 0.24 Tabulated maximum. For nominal thickness or diameter greater than 30 mm, carbon shall not exceed 0.22%. For sections thicker than 100 mm, carbon may be agreed by both parties.
Si 0.55 If silicon is deliberately held down for galvanizing, see the CEV footnotes in the next table.
Mn 1.60 —
P 0.035 For sections and bars the standard allows this maximum to be raised by 0.005% (to 0.040%).
S 0.035 For sections and bars the standard allows this maximum to be raised by 0.005% (to 0.040%).
Nb, V, Ti — Not required additions in Table 1 for Q355. Other alloying elements may be added by agreement and shall be reported on the certificate.
Cr 0.30 —
Ni 0.30 —
Cu 0.40 —
Mo — —
N 0.012 If the supplier guarantees nitrogen, analysis may be omitted. If acid-soluble aluminium is at least 0.015% or total aluminium is at least 0.020%, or other nitrogen-binding elements are added, nitrogen is not restricted and shall be stated on the certificate.
B — —

On every tabulated standard channel the web is well under 30 mm, so the 0.24% carbon maximum applies when the web is the test location. The 0.22% carbon footnote for thickness greater than 30 mm, and the agreement option for sections thicker than 100 mm, remain in the table because a special heavier bar could be agreed.

Q355B Carbon Equivalent for As-Rolled Channels

The carbon equivalent is calculated from the ladle analysis by the standard IIW formula given in GB/T 1591: CEV = C + Mn/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15. Table 2 maxima for as-rolled Q355 (qualities B, C and D share these cells) are shown below. When the web is the test location, every tabulated standard channel sits in the first (0.45%) band.

Nominal thickness or diameter (mm) Maximum CEV (ladle analysis, %)
t ≤ 30 0.45
30 < t ≤ 63 0.47
63 < t ≤ 150 0.47
150 < t ≤ 250 0.49 (for sections and bars the standard allows this maximum to be 0.54%)
250 < t ≤ 400 Not specified for quality B (the 0.49 value in this band applies only to quality D plate).

When silicon is controlled, for example for a hot-dip galvanizing route, and carbon or manganese is raised to keep the tensile properties, the standard allows the tabulated CEV maximum to be increased by 0.02% if silicon is not more than 0.030%, or by 0.01% if silicon is not more than 0.25%. Those increments should appear on the order if they are to be used. This page does not quote other raised CEV figures for thinner bands, because the 0.54% allowance is the one the standard attaches to the >150–250 mm cell for sections and bars.

Q355B Channel Mechanical Properties: Yield, Tensile and +20 °C Impact

Tensile properties of as-rolled Q355 are thickness-dependent. The values below are from GB/T 1591-2018 Tables 7 and 8, using the longitudinal elongation column that applies to sections and bars. For these channels GB/T 706 directs specimens taken under GB/T 2975 to the web, so the relevant thickness is ordinarily the web d. All of the tabulated standard channels have a web of 14.5 mm or less, so they remain in the first (355 MPa / 22%) band when the web is the test location. The later bands are still shown because a thicker special section could be agreed, and because relocating the specimen is a matter for the order, not a habit. For plates, specimens are usually transverse and elongation may be lower — use the Q355B steel plate page for those figures, not this table. When yield is not clearly pronounced, Rp0.2 may be used in place of ReH, as the standard allows.

Nominal thickness or diameter t (mm) Minimum yield ReH (MPa) Tensile strength Rm (MPa) Minimum elongation A, longitudinal (%)
t ≤ 16 355 470–630 22
16 < t ≤ 40 345 470–630 22
40 < t ≤ 63 335 470–630 21
63 < t ≤ 80 325 470–630 20
80 < t ≤ 100 315 470–630 20
100 < t ≤ 150 295 450–600 18
150 < t ≤ 200 285 450–600 17
200 < t ≤ 250 275 450–600 17

Quality B requires a Charpy V-notch absorbed energy at +20 °C of 34 J on a longitudinal specimen, or 27 J if a transverse specimen is agreed. The default is longitudinal. GB/T 1591 requires the impact test when the nominal thickness is not less than 6 mm (or the nominal diameter is not less than 12 mm); for sections, that thickness is the specimen-preparation thickness in GB/T 2975. Several light tabulated channels have a web under 6 mm and therefore sit outside that obligation as written; the remaining tabulated webs are inside it. If a standard 10 mm × 10 mm × 55 mm specimen cannot be prepared, the standard allows a 7.5 mm or 5 mm subsidiary specimen at 75% or 50% of the Table 11 value, with the larger size preferred. The specimen size actually used belongs on the certificate. If the project needs 34 J at 0 °C or at −20 °C, the grade to nominate is Q355C or Q355D, not Q355B.

Delivery Conditions, Inspection and Identification

This product is as-rolled Q355B. GB/T 1591 also defines normalized and thermomechanical Q355 grades; those conditions, and their chemistry tables, must be named if they are required. The inspection document should identify Q355B, the GB/T 1591 edition, the as-rolled delivery condition, the carbon equivalent, the GB/T 706 designation and the edition used for dimensions and mass, the heat number, ladle analysis, and the tensile and impact results against the thickness at the test location, which for these channels is ordinarily the web. Packaging, marks and certificates follow GB/T 2101 in the edition named on the order. A plate certificate, or an H-beam certificate, does not, by itself, identify a channel.

An EN 10204 type 3.1 document is the usual export request; type 3.2 or nominated third-party attendance can be added when the specification requires it. Identification on the product follows the mill’s marking practice and the ordered standards. Length is a matter for the rolling programme and the order.

Weldability and Surface Condition of Q355B Channels

Q355B is a weldable high-strength low-alloy structural steel when thickness, joint design, hydrogen control and the actual carbon equivalent are taken into account. The CEV table above is the starting point; the certificate values and a procedure suited to the thickness are the practical controls. This page does not prescribe a procedure or a preheat chart.

The as-rolled surface is mill scale. A blast class, a paint system, or a hot-dip galvanizing chemistry is an order option, not something implied by the grade name. If galvanizing is planned, the silicon and phosphorus on the heat, the CEV footnotes for controlled silicon, and the processor’s coating specification should be reviewed before production. Surface quality also follows the ordered edition of GB/T 706; special finish requirements belong in the enquiry. Cutting to length, punching, forming or coating can be reviewed when the specification is sent with the enquiry. They are not assumed for every size.

GB/T 706 Shape Tolerances and Theoretical Mass

Dimensional and mass tolerances for these channels are those of GB/T 706, not of GB/T 1591 and not of the GB/T 11263 envelope written for H-sections. This article uses GB/T 706-2016 as the numeric size basis and does not reproduce the millimetre tolerance tables; acceptance is against the edition named on the order. GB/T 706-2026 is the successor edition, with implementation from 1 December 2026.

A delivered 20b will measure close to 200 × 75 × 9 mm within those tolerances, not as a set of exact advertised millimetres. Out-of-square and flange tilt matter for connections. Settlement on theoretical or weighed mass should follow the contract. Theoretical masses in the size table use a density of 7.85 g/cm³; they are not a substitute for a weighed-mass agreement if the order requires one.

Applications and Service Limits

Q355B steel channels are used where a 355 MPa yield class, a +20 °C impact quality and a GB/T 706 channel are accepted:

  • Building frames, plant structures, platforms, stair stringers and general structural fabrication.
  • Machinery bases, skids and support steelwork that actually specify a 355 MPa as-rolled grade rather than Q235B.
  • Export packages that compare the grade with S355JR H-beam or with A572 Grade 50 plate, provided each line keeps its own material standard and shape system.

It is not specified here for pressure equipment, for nuclear safety-related components, or for structures whose specification requires a lower impact-test temperature or a normalized or thermomechanical delivery condition. Durability comes from the coating or fire-protection system, not from the grade name. Weathering or marine exposure needs an agreed protection system, not bare Q355B.

Q355B Channel Compared with Q235B, S355JR and A572 Grade 50

Q355B and Q235B can share the GB/T 706 channel series, but they are different material standards and different yield classes. Q235B is specified to GB/T 700, with a 235 MPa yield class, a looser phosphorus and sulphur table, no published CEV maximum, and a 27 J longitudinal impact requirement at +20 °C. An enquiry that says only “Chinese channel” is incomplete.

S355JR H-beam is a near-equivalent in yield class, but a European channel in that grade would be a UPN, UPE or PFC, not a Chinese 16a or 20b, unless a mill has a documented special combination, and its impact requirement is 27 J rather than 34 J longitudinal. ASTM A572 Grade 50 is a 50 ksi (345 MPa) grade on a different shape system. Dual certification is possible only when the delivered piece meets every requirement of each named standard, including chemistry, tests, dimensions and tolerances. Q355B H-beam and Q355B plate share the material grade, not the section.

A Q355B angle to GB/T 706, and a Q235B channel to the same dimensional standard, will be linked here once those pages are published; those product URLs are not pre-linked.

Near-Equivalents: Not Automatic Substitutes

The comparisons below are for orientation. They are not a licence to substitute one grade or one shape for another on a contract or an inspection certificate.

Grade / designation Standard Relationship to Q355B channel Caution
Q345B (former designation) Earlier editions of GB/T 1591 GB/T 1591-2018 replaced the Q345 steel grade with Q355. Appendix A maps as-rolled Q355B to the former Q345B. Do not treat a historical Q345B certificate as automatically meeting the 2018 Q355B table. Name the 2018 grade and edition on new orders.
Q355C / Q355D (as-rolled) GB/T 1591-2018 Same 355 MPa yield class. C is tested at 0 °C (34 J longitudinal) and D at −20 °C. Tighter phosphorus and sulphur, and a thickness-split carbon table. Not interchangeable with B on a +20 °C specification.
Q355N / Q355M GB/T 1591-2018 Same yield class in the normalized or thermomechanical conditions, with their own chemistry and CEV tables. Do not certify as-rolled Q355B as Q355N or Q355M unless the actual delivery condition and tables are met.
Q235B GB/T 700; a GB/T 706 channel may be certified to Q235B when that is the order A lower-strength Chinese carbon-steel comparison on the same GB/T 706 channel series. Q235B is not Q355B. It has no published CEV cap and a 27 J, not 34 J longitudinal, impact requirement at +20 °C.
S355JR EN 10025-2; dimensions EN 10365 / tolerances EN 10279 for channels A comparable 355 MPa European grade with a +20 °C impact quality, usually as UPN, UPE or PFC when the product is a channel. S355JR impact is 27 J, not 34 J longitudinal. Chemistry, CEV rules and the European channel system all differ. A UPN 200 is not a Chinese 20b.
ASTM A572 Grade 50 ASTM A572/A572M; American channel dimensions ASTM A6/A6M A common 50 ksi (345 MPa) high-strength low-alloy comparison in export enquiries. Yield class, chemistry and the C or MC shape system differ. Not an automatic substitute.

Sourcing Q355B Steel Channels from SHH STEEL

SHH STEEL supplies Q355B steel channels as an export trading house, coordinating mill production and project procurement. The useful part of that model is to keep the material edition and the as-rolled Q355B condition (GB/T 1591-2018, rather than a former Q345B call or an N/M condition) distinct from the shape edition (GB/T 706-2016 as the numeric basis here, or the successor edition when that is what the order names), to apply the yield and CEV bands to the web thickness rather than the channel depth, and to align the inspection document before a rolling programme is committed.

Sections can be sourced from mills that SHH STEEL buys from, including Masteel, Rizhao Steel, Laiwu (Shandong Steel Laiwu) and Tung Ho Steel, among others when the programme matches the order. Those mills do not each roll every Table A.2 size in Q355B. Mid-range models such as 10, 16a and 20b are the usual core; the light 5 and 6.3 rows and the 36 and 40 rows are confirmed per line.

The same enquiry can also cover angles, H-sections, or European, American or Japanese designations, provided each line states its material standard, shape standard, delivery condition and size. If cutting, punching, forming or a coating system is required, include that specification for review. Export packing and container loading can be arranged to the packing list agreed for the shipment.

Q355B Steel Channel FAQs

Is Q355B the same as Q345B?
Q355B is the current as-rolled quality-B grade in GB/T 1591-2018; that edition replaced the Q345 designation with Q355. Appendix A maps Q355B to the former Q345B, but a historical Q345B certificate should not be treated as automatically meeting the 2018 tables. New orders should name Q355B, the as-rolled condition, and the 2018 edition or the edition on the contract.
Does the 355 MPa yield apply to every Q355B channel in the table?
For these channels GB/T 706 directs specimens taken under GB/T 2975 to the web, so the thickness band is ordinarily the web thickness d, not the overall depth and not automatically the flange thickness. Every tabulated standard channel has a web of 14.5 mm or less, so the first (355 MPa / 22%) band applies when the web is the test location. The later bands remain in the mechanical table for a thicker special section or a relocated specimen written on the order.
Is the impact requirement 27 J, like S355JR, and does it apply to every size?
No. As-rolled Q355B requires 34 J on a longitudinal specimen at +20 °C, or 27 J if a transverse specimen is agreed. S355JR uses 27 J at +20 °C under EN 10025-2. GB/T 1591 requires the impact test when the nominal thickness is not less than 6 mm; for these channels that thickness is ordinarily the web. Several light tabulated channels have a web under 6 mm and therefore sit outside that obligation as written.
Which edition of GB/T 706 is used for the size table?
The size table uses GB/T 706-2016 as the numeric basis and is the complete Table A.2 series of 41 sizes, from model 5 (50×37×4.5) to model 40c (400×104×14.5). GB/T 706-2026 is the successor edition, with implementation from 1 December 2026. The edition of GB/T 706 named on the order governs dimensional acceptance.
Which standards should appear on the inspection document?
At least GB/T 1591 and its edition, the grade Q355B, the as-rolled delivery condition, the carbon equivalent, the GB/T 706 designation and the edition used for dimensions and mass, ladle analysis, and tensile and impact results against the thickness at the test location, ordinarily the web. Packaging, marks and certificates follow GB/T 2101. A plate or H-beam certificate does not, by itself, identify a channel.

Request a Quotation for GB/T 706 Q355B Steel Channel

GB/T 706 Q355B steel channel is a taper-flange Chinese channel in as-rolled Q355B, with 355 MPa minimum yield in the first thickness band and a 34 J longitudinal impact requirement at +20 °C. Nominate the GB/T 706 designation (for example 16a, 20b or [200×75×9), the material to GB/T 1591-2018 as-rolled Q355B (or the edition on the order), and the carbon equivalent basis. The size table uses GB/T 706-2016 as the numeric basis; GB/T 706-2026 is the successor edition, with implementation from 1 December 2026; the ordered edition governs. Send the size list, edition, condition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X