GB/T 11251 35CrMo Alloy Steel Plate
What is GB/T 11251 Grade 35CrMo plate?
GB/T 11251 35CrMo Alloy Steel Plate is alloy structural steel plate and strip purchased to GB/T 11251-2025. Grade 35CrMo is not one of the fourteen grades listed in Table 1. It may be supplied under that plate specification because clause 6.1.1 requires chemistry to GB/T 3077 and clause 6.2.1.2 sets mechanical properties of other grades by agreement.
35CrMo carries more carbon than 30CrMo and less than 42CrMo. It is selected when the design wants more hardenability than 30CrMo without moving to the 42CrMo or 4140 carbon level. It is not a drop-in for ASTM A829 4140.
Single-rolled plate is usually supplied high-temperature tempered unless another condition is agreed. Because Table 1 does not list 35CrMo, any tensile, hardness or toughness acceptance criteria must be written on the contract.
SHH STEEL produces and exports GB/T 11251-2025 Grade 35CrMo plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry. This grade belongs to our Alloy Steel Plates range under GB/T 11251.
Material specification for GB/T 11251 Grade 35CrMo
The items below follow GB/T 11251-2025. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.
| Parameter | Detail |
|---|---|
| Standard | GB/T 11251-2025, Alloy structural steel plate, sheet and strip. Published 31 October 2025 and implemented 1 May 2026. It replaces GB/T 11251-2020 and GB/T 37601-2019 |
| Grade designation | Grade 35CrMo, chromium-molybdenum alloy structural steel, not listed in Table 1 |
| Product forms in the standard | Single-rolled hot-rolled plate, nominal thickness 3.0 mm to 250 mm; and continuous-rolled plate and strip, nominal thickness not greater than 25.4 mm (wide strip and cut plate or slit strip 600 mm wide or more, and narrow strip and cut plate under 600 mm) |
| Chemical composition | Shall comply with GB/T 3077 (clause 6.1.1). This grade is not listed in Table 1. Optional phosphorus or sulfur variants may be agreed under clause 6.1.1. Product analysis shall meet GB/T 222 |
| Single-rolled delivery | High-temperature tempered as the usual condition; annealed, normalized, normalized and tempered, or quenched and tempered by agreement. Normalizing rolling may replace normalizing if the normalized mechanical requirements can be met |
| Continuous-rolled delivery | As-rolled; heat treatment by agreement. If spheroidize-annealed, surface hardness shall meet GB/T 3077. Tensile tests on continuous-rolled material are by agreement |
| Annealed single-rolled mechanics | Table 1 does not list Grade 35CrMo. Clause 6.2.1.2 says mechanical properties of grades other than those in Table 1 are determined by agreement between the purchaser and the manufacturer. Do not copy a neighbouring Table 1 tensile band onto this grade |
| Dimensions | Single-rolled plate to GB/T 709-2019, thickness tolerance class A. Wide strip and cut plate or slit strip to GB/T 709-2019 Table 4 thickness tolerances; flatness by agreement. Narrow strip and cut plate to Annex A |
| Ultrasonic testing | Single-rolled plate 6 mm thick or thicker shall be tested to GB/T 2970-2016 Class II unless another method and class are agreed |
| Our supply | We produce and export Grade 35CrMo to the GB/T 11251-2025 form, delivery condition, dimensions and extra tests agreed on the order |
Chemical composition of GB/T 11251 Grade 35CrMo
GB/T 11251-2025 clause 6.1.1 requires the grade and chemical composition to comply with GB/T 3077. Grade 35CrMo is not listed in Table 1 of the 2025 plate specification. It is supplied as plate or strip when the purchase order names it under GB/T 11251, with chemistry taken from GB/T 3077. The melt-analysis figures below are published GB/T 3077-2015 values for Grade 35CrMo. They are not a separate chemistry table printed inside GB/T 11251-2025 itself, and they must not be read as an older GB/T 11251-2020 or GB/T 37601-2019 reprint labelled as 2025. Product-analysis tolerances shall meet GB/T 222; use the applicable GB/T 222 limits for acceptance.
| Element | Reference melt analysis (wt. %) |
|---|---|
| Carbon (C) | 0.32-0.40 |
| Silicon (Si) | 0.17-0.37 |
| Manganese (Mn) | 0.40-0.70 |
| Chromium (Cr) | 0.80-1.10 |
| Molybdenum (Mo) | 0.15-0.25 |
Phosphorus and sulfur depend on the GB/T 3077 quality class ordered: ordinary quality steel, high-quality steel designated by adding A, or extra-quality steel designated by adding E. Published secondary tables sometimes round those maxima; confirm the class and the limits on the mill test certificate. GB/T 11251-2025 also allows, by agreement on the contract, sulfur of 0.015% to 0.035% or not greater than 0.005%, or phosphorus not greater than 0.015%. Residual elements that are not specified alloying additions are limited by GB/T 3077.
Mechanical properties and optional tests
Grade 35CrMo is not listed in GB/T 11251-2025 Table 1. Clause 6.2.1.2 states that, for single-rolled plate, the mechanical properties of grades other than those in Table 1 are determined by agreement between the purchaser and the manufacturer. The same clause also sends thickness greater than 100 mm to agreement, even for Table 1 grades. This page therefore does not publish annealed tensile strength or elongation numbers for Grade 35CrMo. Neighbouring Table 1 bands must not be copied onto this grade, and they are not implied guarantees.
When single-rolled plate is delivered high-temperature tempered, clause 6.2.1.1 requires surface hardness in accordance with GB/T 3077. This page does not reprint a numeric hardness table from the bar specification. Normalized, normalized-and-tempered and quenched-and-tempered properties are contractual. The Table 1 normalized rule — elongation not less than Table 1, with the tensile upper limit allowed 50 MPa higher — applies to Table 1 grades; it is not used here as an automatic 35CrMo plate minimum.
Continuous-rolled plate and strip may be tensile-tested only by agreement. Quenched-and-tempered tensile and yield figures published for GB/T 3077 bars are not automatic GB/T 11251 plate minima and are not used on this page.
Delivery conditions for GB/T 11251 Grade 35CrMo
GB/T 11251-2025 distinguishes two product routes:
- Single-rolled plate is usually delivered high-temperature tempered. Annealed, normalized, normalized and tempered, or quenched and tempered supply may be agreed and written on the contract. Normalizing rolling may replace normalizing if the normalized mechanical requirements can be guaranteed.
- Continuous-rolled plate and strip are delivered as-rolled unless a heat-treatment condition is agreed. If they are spheroidize-annealed, surface hardness shall meet GB/T 3077.
We produce and export Grade 35CrMo to the agreed route and condition. An enquiry that only says “35CrMo plate” is incomplete, because high-temperature tempered, annealed, normalized and quenched-and-tempered plate are not interchangeable supply states, single-rolled plate is not the same product as continuous-rolled plate or strip, and this grade has no Table 1 default tensile package.
Welding and thermal cutting
35CrMo is a higher-carbon chromium-molybdenum grade than 20CrMo or 30CrMo. The heat-affected zone can harden more readily, so welding and thermal cutting need more control. It is generally less weld-friendly than 15CrMo or 20CrMo. Preheat, interpass temperature and any post-weld heat treatment depend on thickness, joint restraint and the qualified procedure. Qualify cutting and welding procedures to the project specification, the ordered delivery condition and the actual thickness.
Thermal cutting can harden the adjacent material. That heat-affected zone should be considered, and removed where later forming or welding requires it.
Form, dimensions and inspection
Single-rolled plate dimensions, shape and mass tolerances follow GB/T 709-2019, with thickness tolerance class A unless another class is agreed. Wide strip and plate or slit strip cut from it follow GB/T 709-2019, using the thickness tolerances in Table 4 of that standard; flatness is agreed on the contract. Narrow strip and plate cut from it follow Annex A of GB/T 11251-2025. Other sizes and tolerances may be agreed.
Single-rolled plate 6 mm thick or thicker shall receive ultrasonic testing to GB/T 2970-2016 Class II unless another standard and class are written on the order. For stamping, single-rolled plate not thicker than 10 mm shall pass a 180° bend test with former diameter D = 2a.
Applications and specification limits
We produce and export this grade for heavier-duty engineering parts that need more hardenability than 30CrMo without stepping all the way to 42CrMo. Cut parts are often quenched and tempered later when the contract calls for that route. That later heat treatment is not an automatic as-delivered 11251 guarantee.
35CrMo is not a fastener-standard listing on this page, and it is not a drop-in for ASTM A829 4140.
GB/T 11251 is an alloy structural plate and strip specification. It is not a boiler or pressure-vessel specification.
Compare GB/T 11251 35CrMo with other steel plates
GB/T 11251 Grade 35CrMo is alloy structural plate and strip under the 2025 Chinese plate specification. It is not a Table 1 grade. The comparison below uses other plates we already publish. These grades are related by engineering use or chemistry family, not equivalents.
| Material | Alloy / type | Delivery condition | Mechanical requirements | Typical service | Substitution limit |
|---|---|---|---|---|---|
| GB/T 11251 Grade 35CrMo (this plate) | Chromium-molybdenum alloy structural plate and strip under GB/T 11251-2025, supplied by agreement rather than as a Table 1 grade | Single-rolled: high-temperature tempered unless annealed, N, NT or QT is agreed. Continuous-rolled: as-rolled unless heat treated by agreement | Not listed in Table 1. Mechanical properties are by agreement under clause 6.2.1.2. High-temperature tempered plate is ordered to GB/T 3077 hardness, without a numeric hardness table on this page | Heavier-duty shafts, connecting parts and other engineering components after an agreed heat treatment | Not a drop-in for ASTM A829 4140 or 42CrMo, and not a pressure-vessel plate |
| ASTM A829 4140 Alloy Steel Plate | Chromium-molybdenum alloy structural plate under ASTM A829/A829M-25, usually ordered by heat chemistry. Manufacturer heat-analysis windows on that page: C 0.36–0.44, Mn 0.75–1.00, Si 0.15–0.35, Cr 0.80–1.10 and Mo 0.15–0.25 | ASTM A829/A829M-25 permits AR, A, N, NT or QT; specify the required condition. | No automatic as-delivered strength package; tensile or hardness only if specified and compatible with analysis, condition and thickness | Machinery and general engineering parts, often heat treated after cutting | Related Cr-Mo family, not a match. 35CrMo carbon is 0.32-0.40 against 4140 at 0.36-0.44; manganese is 0.40-0.70 against 0.75-1.00; chromium is 0.80-1.10 against 0.80-1.10 |
| ASTM A829 4130 Alloy Steel Plate | Chromium-molybdenum alloy structural plate under ASTM A829/A829M-25, usually ordered by heat chemistry. Manufacturer heat-analysis windows on that page: C 0.28–0.33, Mn 0.40–0.60, Si 0.15–0.35, Cr 0.80–1.10 and Mo 0.15–0.25 | Usually ordered by chemistry; tensile only if specified and compatible | No automatic as-delivered strength package | Engineering plate with a lower carbon window than Grade 4140 in the same family | Higher carbon than 4130 (0.32-0.40 against 0.28-0.33). 4130 is the closer pairing for 30CrMo, not for 35CrMo |
| GB/T 713 15CrMoR Steel Plate | 1.25Cr-0.5Mo boiler and pressure-vessel plate under GB/T 713.2-2023, not an engineering-plate GB/T 11251 grade | Vessel-plate delivery as specified for 15CrMoR (from our 15CrMoR page) | Strength-graded on our 15CrMoR page: yield 295 MPa at 6–60 mm and tensile 450–590 MPa | Boilers and pressure vessels | 15CrMoR is a GB/T 713 vessel plate with published yield and tensile values. 35CrMo is 11251 engineering plate without a Table 1 tensile package |
Related published ranges: Alloy Steel Plates.
Equivalent and related grades by country
The designations below are near equivalents or related chemistry-family grades, not certified or automatic equivalents. Chemistry windows, product form, delivery condition and tests must match the project specification before a substitution is considered. Grades without a live page on this site are shown as plain text unless a live contrast page is named.
| Country / region | Standard | Grade | Similarity and key differences | Substitution caveat |
|---|---|---|---|---|
| China | GB/T 11251-2025 | 35CrMo | This plate. Chromium-molybdenum alloy structural plate and strip supplied under the 2025 specification by agreement, not listed in Table 1. | This product |
| China | GB/T 3077-2015 | 35CrMo | Chemistry reference (bar specification). Published melt analysis: C 0.32-0.40, Si 0.17-0.37, Mn 0.40-0.70, Cr 0.80-1.10, Mo 0.15-0.25. | Do not treat GB/T 3077 bar quenched-and-tempered figures as GB/T 11251 plate minima. |
| United States | ASTM A829/A829M-25 | Grade 4140 | Related higher-carbon chromium-molybdenum plate, not a match. Manufacturer 4140 heat analysis: C 0.36-0.44, Mn 0.75-1.00, Si 0.15-0.35, Cr 0.80-1.10, Mo 0.15-0.25, against 35CrMo C 0.32-0.40 and Mn 0.40-0.70. | Different specification. Restate product form, delivery condition and tests rather than substituting on chemistry-family resemblance. |
| United States | ASTM A829/A829M-25 | Grade 4130 | Lower-carbon related plate. Manufacturer 4130 carbon is 0.28-0.33 against 35CrMo at 0.32-0.40. | Different specification. Restate product form, delivery condition and tests rather than substituting on chemistry-family resemblance. |
| Japan | JIS G 4053 | SCM435 | Published heat analysis: C 0.33-0.38, Si 0.15-0.35, Mn 0.60-0.90, Cr 0.90-1.20, Mo 0.15-0.30. Carbon sits inside the 35CrMo window; manganese, chromium and the molybdenum upper limit are higher, and 35CrMo carbon extends to 0.40. | JIS G 4053 is a machine-structural steel specification, not a plate specification. Do not order plate to the JIS title alone. |
No AISI/SAE 4135 plate page is published on this site, and this article does not invent an A829 4135 listing. European 34CrMo4 is often listed against both 30CrMo and 35CrMo; no official 34CrMo4 table is cited here.
Why choose SHH STEEL for GB/T 11251 Grade 35CrMo
- We produce and export GB/T 11251-2025 Grade 35CrMo alloy structural steel plate
- We review the enquiry for edition, grade, product route, delivery condition, dimensions and extra tests
- We keep this by-agreement grade distinct from Table 1 guaranteed mechanics and from GB/T 3077 bar figures
- We match documentation to what the purchase order requires
How to enquire for GB/T 11251 35CrMo plate
| Item | What to specify |
|---|---|
| Standard and grade | GB/T 11251-2025 Grade 35CrMo |
| Product route | Single-rolled plate, or continuous-rolled plate or strip |
| Delivery condition | High-temperature tempered, annealed, normalized, normalized and tempered, quenched and tempered, or as-rolled for continuous-rolled material |
| Dimensions | Required thickness, width and length; we confirm production and export feasibility against the enquiry |
| Chemistry | Melt analysis to GB/T 3077, including any A or E quality class; request product analysis to GB/T 222 only if needed; state any agreed phosphorus or sulfur variant |
| Mechanical tests | State the agreed tensile, hardness, toughness or other acceptance criteria. Table 1 annealed values do not apply to this grade |
| Other tests | Ultrasonic class if different from the standard Class II rule, bend testing for stamping, decarburization or inclusion rating only when written on the order |
| Documentation | State the inspection document type required by the project |
FAQ
-
Is GB/T 11251 35CrMo ordered only by chemistry?
- Chemistry shall comply with GB/T 3077. Grade 35CrMo is not listed in Table 1, so the specification does not publish annealed tensile and elongation values for it. Write the tensile, hardness or toughness criteria you need on the contract. High-temperature tempered single-rolled plate is ordered to GB/T 3077 hardness rather than to a Table 1 tensile band.
-
Is GB/T 11251 35CrMo a substitute for 42CrMo or ASTM A829 4140?
- No. 35CrMo carbon is 0.32-0.40, below 42CrMo at 0.38-0.45 and below the manufacturer 4140 window of 0.36-0.44. Manganese also differs from 4140 (0.40-0.70 against 0.75-1.00). Choose the grade the design actually specifies.
-
Does Table 1 apply to this grade?
- No. Table 1 of GB/T 11251-2025 lists fourteen grades; 35CrMo is not among them. Clause 6.2.1.2 sends the mechanical properties of other grades to agreement. Do not copy a neighbouring Table 1 tensile or elongation figure onto 35CrMo. The normalized allowance of a 50 MPa higher tensile upper limit is a Table 1 rule, not an automatic value for this grade.
-
Did GB/T 11251-2025 replace GB/T 37601?
- Yes. The 2025 edition replaces GB/T 11251-2020 and GB/T 37601-2019 and integrates the continuous-rolled content. Do not order this plate to the withdrawn 37601 specification as if it were still current.
-
What should a quotation enquiry include?
- The ordered GB/T 11251 edition, Grade 35CrMo, single-rolled or continuous-rolled route, delivery condition, thickness by width by length, quantity, the agreed mechanical acceptance criteria (because Table 1 does not apply), any extra chemical tests, any NDE, and the inspection document required by the project.
Request a quotation
Contact SHH STEEL for a quotation for GB/T 11251-2025 Grade 35CrMo alloy steel plate. Please include your required quantity, plate thickness, width and length, whether you need single-rolled plate or continuous-rolled plate or strip, delivery destination and preferred delivery schedule so we can review your production and export requirements.
Specify the delivery condition and the mechanical tests you need, because this grade has no Table 1 default tensile package. If your project requires tensile, hardness, toughness or ultrasonic testing beyond the standard rules, include the acceptance criteria and the inspection document required.
If you are comparing 35CrMo with 42CrMo or with ASTM A829 4140, say so on the enquiry. We will review the differences in product form, chemistry and supply condition rather than assume that related grades are interchangeable.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.
Contact: admin@steelspecs.com