GB/T 11251 30CrMnSi Alloy Steel Plate | GB/T 11251 Alloy Steel - SHH STEEL

GB/T 11251 30CrMnSi Alloy Steel Plate

GB/T 11251 30CrMnSi is chromium-manganese-silicon alloy structural steel plate under GB/T 11251-2025, Alloy structural steel plate, sheet and strip. The 2025 edition replaces GB/T 11251-2020 and GB/T 37601-2019. Grade 30CrMnSi is listed in Table 1 for annealed single-rolled plate not thicker than 100 mm. Chemical composition is specified by reference to GB/T 3077. SHH STEEL produces and exports Grade 30CrMnSi alloy steel plate to the specified delivery condition and project requirements.
Equivalent Grades:
Related grades: 20CrMnSi, 25CrMnSi, 35CrMnSi. Different chemistry and properties; not automatic substitutes.
Heat Treatment
Single-rolled: high-temperature tempered, annealed, normalized, normalized and tempered, or quenched and tempered. Continuous-rolled: as-rolled or heat-treated.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is GB/T 11251 Grade 30CrMnSi plate?

GB/T 11251 30CrMnSi Alloy Steel Plate is alloy structural steel plate and strip purchased to GB/T 11251-2025. Grade 30CrMnSi is one of the fourteen grades for which the 2025 edition publishes annealed single-rolled tensile and elongation values in Table 1. When agreed on the contract, clause 6.2.1.5 also allows a specimen quench-and-temper test to Table 2 for this grade and for 25CrMnSi only.

The 2025 edition is a plate and strip specification. Chemical composition shall comply with GB/T 3077, used here as the chemistry reference, not as the delivery specification. Adding A after the grade name orders the high-quality class of the same base grade; it is not a separate Table 1 row.

Single-rolled plate is usually supplied high-temperature tempered unless another condition is agreed. Table 1 tensile values apply only to annealed single-rolled plate not thicker than 100 mm. Table 2 specimen values are not automatic as-delivered plate minima.

SHH STEEL produces and exports GB/T 11251-2025 Grade 30CrMnSi plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry. This grade belongs to our Alloy Steel Plates range under GB/T 11251.

Material specification for GB/T 11251 Grade 30CrMnSi

The items below follow GB/T 11251-2025. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard GB/T 11251-2025, Alloy structural steel plate, sheet and strip. Published 31 October 2025 and implemented 1 May 2026. It replaces GB/T 11251-2020 and GB/T 37601-2019
Grade designation Grade 30CrMnSi, chromium-manganese-silicon alloy structural steel plate listed in GB/T 11251-2025 Table 1
Product forms in the standard Single-rolled hot-rolled plate, nominal thickness 3.0 mm to 250 mm; and continuous-rolled plate and strip, nominal thickness not greater than 25.4 mm (wide strip and cut plate or slit strip 600 mm wide or more, and narrow strip and cut plate under 600 mm)
Chemical composition Shall comply with GB/T 3077. Optional phosphorus or sulfur variants may be agreed under clause 6.1.1. Product analysis shall meet GB/T 222
Single-rolled delivery High-temperature tempered as the usual condition; annealed, normalized, normalized and tempered, or quenched and tempered by agreement. Normalizing rolling may replace normalizing if the normalized mechanical requirements can be met
Continuous-rolled delivery As-rolled; heat treatment by agreement. If spheroidize-annealed, surface hardness shall meet GB/T 3077. Tensile tests on continuous-rolled material are by agreement
Annealed single-rolled mechanics Table 1 applies to Grade 30CrMnSi at nominal thickness not greater than 100 mm. Thickness over 100 mm, and grades other than Table 1, are by agreement
Dimensions Single-rolled plate to GB/T 709-2019, thickness tolerance class A. Wide strip and cut plate or slit strip to GB/T 709-2019 Table 4 thickness tolerances; flatness by agreement. Narrow strip and cut plate to Annex A
Ultrasonic testing Single-rolled plate 6 mm thick or thicker shall be tested to GB/T 2970-2016 Class II unless another method and class are agreed
Our supply We produce and export Grade 30CrMnSi to the GB/T 11251-2025 form, delivery condition, dimensions and extra tests agreed on the order

Chemical composition of GB/T 11251 Grade 30CrMnSi

GB/T 11251-2025 requires the grade and chemical composition to comply with GB/T 3077. The melt-analysis figures below are published GB/T 3077-2015 values for Grade 30CrMnSi. They are not a separate chemistry table printed inside GB/T 11251-2025 itself, and they must not be read as an older GB/T 11251-2020 or GB/T 37601-2019 reprint labelled as 2025. Product-analysis tolerances shall meet GB/T 222; use the applicable GB/T 222 limits for acceptance.

Element Reference melt analysis (wt. %)
Carbon (C) 0.28-0.34
Silicon (Si) 0.90-1.20
Manganese (Mn) 0.80-1.10
Chromium (Cr) 0.80-1.10

Phosphorus and sulfur depend on the GB/T 3077 quality class ordered: ordinary quality steel, high-quality steel designated by adding A, or extra-quality steel designated by adding E. Published secondary tables sometimes round those maxima; confirm the class and the limits on the mill test certificate. GB/T 11251-2025 also allows, by agreement on the contract, sulfur of 0.015% to 0.035% or not greater than 0.005%, or phosphorus not greater than 0.015%. Residual elements that are not specified alloying additions are limited by GB/T 3077.

Mechanical properties and optional tests

For annealed single-rolled plate of Grade 30CrMnSi with nominal thickness not greater than 100 mm, GB/T 11251-2025 Table 1 specifies tensile strength Rm of 550-750 MPa and elongation A of not less than 19 %. For nominal thickness greater than 20 mm and not greater than 100 mm, elongation may be reduced by 0.25 % (absolute) for each 1 mm increase in thickness, but by not more than 5 % (absolute).

When single-rolled plate is delivered normalized, elongation shall still meet the Table 1 value and the upper limit of tensile strength may be 50 MPa higher than Table 1. High-temperature tempered single-rolled plate is ordered to surface hardness in accordance with GB/T 3077, not to the annealed Table 1 tensile band. Normalized-and-tempered and quenched-and-tempered single-rolled plate have mechanical properties agreed on the contract. Thickness greater than 100 mm is also by agreement.

Continuous-rolled plate and strip may be tensile-tested only by agreement; those results are not Table 1 values. Quenched-and-tempered GB/T 3077 bar figures must not be read as automatic GB/T 11251 plate minima.

Separately from Table 1, clause 6.2.1.5 of GB/T 11251-2025 allows Grade 30CrMnSi single-rolled plate, when buyer and supplier agree and write it on the contract, to be assessed by a specimen quench-and-temper test to Table 2. Table 2 recommends a specimen quench at 860-900 °C in oil and a temper at 470-570 °C in water or oil. It then lists tensile strength Rm of 1080 MPa, elongation A of 10 % and impact energy KU2 of 39 J. The opened 2025 reprint does not print a greater-than-or-equal-to mark on those three Table 2 figures, unlike the Table 1 elongation column. Clause 6.2.1.5 requires the specimen results to comply with Table 2 for nominal thickness not greater than 30 mm; thicker plate is by agreement. These specimen values are not automatic as-delivered plate minima, and they are not GB/T 3077 bar quenched-and-tempered figures.

Delivery conditions for GB/T 11251 Grade 30CrMnSi

GB/T 11251-2025 distinguishes two product routes:

  • Single-rolled plate is usually delivered high-temperature tempered. Annealed, normalized, normalized and tempered, or quenched and tempered supply may be agreed and written on the contract. Normalizing rolling may replace normalizing if the normalized mechanical requirements can be guaranteed.
  • Continuous-rolled plate and strip are delivered as-rolled unless a heat-treatment condition is agreed. If they are spheroidize-annealed, surface hardness shall meet GB/T 3077.

We produce and export Grade 30CrMnSi to the agreed route and condition. An enquiry that only says “30CrMnSi plate” is incomplete, because high-temperature tempered, annealed, normalized and quenched-and-tempered plate are not interchangeable supply states, and single-rolled plate is not the same product as continuous-rolled plate or strip.

Welding and thermal cutting

Chromium-manganese-silicon 30CrMnSi plate should be welded to a procedure suited to the silicon level, thickness and delivery condition. Preheat is commonly considered as thickness and restraint increase. Preheat, interpass temperature and any post-weld heat treatment depend on thickness, joint restraint and the qualified procedure. Qualify cutting and welding procedures to the project specification, the ordered delivery condition and the actual thickness.

Thermal cutting can harden the adjacent material. That heat-affected zone should be considered, and removed where later forming or welding requires it.

Form, dimensions and inspection

Single-rolled plate dimensions, shape and mass tolerances follow GB/T 709-2019, with thickness tolerance class A unless another class is agreed. Wide strip and plate or slit strip cut from it follow GB/T 709-2019, using the thickness tolerances in Table 4 of that standard; flatness is agreed on the contract. Narrow strip and plate cut from it follow Annex A of GB/T 11251-2025. Other sizes and tolerances may be agreed.

Single-rolled plate 6 mm thick or thicker shall receive ultrasonic testing to GB/T 2970-2016 Class II unless another standard and class are written on the order. For stamping, single-rolled plate not thicker than 10 mm shall pass a 180° bend test with former diameter D = 2a.

Applications and specification limits

We produce and export this grade for general engineering and machinery parts cut from plate and later heat treated to a stated cycle, including welded fabrications where a chromium-manganese-silicon chemistry is specified. An order written as 30CrMnSiA is the high-quality class of this base grade, not a different Table 1 listing.

As-rolled, high-temperature tempered, annealed and quenched-and-tempered plate do not machine or form at the same strength. A Table 2 specimen test, if agreed, does not by itself define the as-delivered plate condition.

GB/T 11251 is an alloy structural plate and strip specification. It is not a boiler or pressure-vessel specification such as GB/T 713.

Compare GB/T 11251 30CrMnSi with other steel plates

GB/T 11251 Grade 30CrMnSi is alloy structural plate and strip under the 2025 Chinese plate specification. The comparison below uses other plates we already publish. These grades are related by engineering use, not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
GB/T 11251 Grade 30CrMnSi (this plate) Chromium-manganese-silicon alloy structural plate and strip under GB/T 11251-2025, chemistry by reference to GB/T 3077 Single-rolled: high-temperature tempered unless annealed, N, NT or QT is agreed. Continuous-rolled: as-rolled unless heat treated by agreement Annealed single-rolled plate ≤ 100 mm: Rm 550-750 MPa and A ≥ 19 % (Table 1). Optional Table 2 specimen QT values only if clause 6.2.1.5 is agreed Engineering and machinery parts, including welded fabrications, often heat treated after cutting Not 30CrMnSiA as a separate Table 1 grade, not Grade 25CrMnSi or 35CrMnSi, and not a 100 ksi QT structural grade
ASTM A829 4140 Alloy Steel Plate Chromium-molybdenum alloy structural plate under ASTM A829/A829M, usually ordered by heat chemistry ASTM A829/A829M-25 permits AR, A, N, NT or QT; specify the required condition. No automatic as-delivered strength package; tensile or hardness only if specified and compatible Machinery and general engineering parts, often heat treated after cutting Related alloy structural plate, not a GB/T 11251 equivalent and not a chromium-only or manganese grade substitute
ASTM A514 Grade B Quenched-and-tempered alloy structural plate; chemistry includes chromium, molybdenum, vanadium, titanium and boron Quenched and tempered Strength-graded: to 32 mm, yield 100 ksi / 690 MPa min and tensile 110-130 ksi / 760-895 MPa (from our A514 Grade B page). Maximum thickness for Grade B is 1¼ in / 32 mm Welded bridges and other structures that specify A514 QT plate Not a substitute for chemistry-referenced GB/T 11251 engineering plate
ASTM A572 Grade 50 High-strength low-alloy structural plate, microalloyed with niobium and vanadium Hot-rolled or controlled-rolled Strength-graded: minimum yield 345 MPa and tensile 450 MPa minimum (from our A572 Grade 50 page) Bridges, buildings, construction equipment, transmission towers and heavy machinery frames Not an alloy engineering plate of the GB/T 11251 type

Related published ranges: Structural Steel Plates, ASTM A514/A514M and ASTM A572/A572M.

Equivalent and related grades by country

The designations below are near equivalents or related chemistry-family grades, not certified or automatic equivalents. Chemistry windows, product form, delivery condition and tests must match the project specification before a substitution is considered. Grades without a live page on this site are shown as plain text unless a live contrast page is named.

Country / region Standard Grade Similarity and key differences Substitution caveat
China GB/T 11251-2025 30CrMnSi This plate and strip specification. Table 1 lists annealed single-rolled tensile and elongation values. Clause 6.2.1.5 also names this grade for an optional Table 2 specimen quench-and-temper test. This product
China GB/T 3077-2015 30CrMnSi The chemistry source cited by GB/T 11251-2025. GB/T 3077 is not a plate specification. Do not treat a 3077 bar enquiry as a 11251 plate order without restating product form, condition and tests.
China GB/T 3077 quality class 30CrMnSiA The high-quality (A) class of the same base grade, not an extra Table 1 row. Order the quality class on the contract rather than treating A as a separate plate SKU.
China GB/T 11251-2025 Table 1 20CrMnSi, 25CrMnSi and 35CrMnSi Related chromium-manganese-silicon plate grades in the same specification. They do not all have product pages on this site yet. Related grades, not automatic substitutes.
United States, Europe and Japan — — No separately verified dedicated plate counterpart was opened for this page. Do not assume a local bar designation is a GB/T 11251 plate equivalent.

Grades 20CrMnSi, 25CrMnSi and 35CrMnSi are related Table 1 grades, not substitutes, and do not all have product pages on this site yet.

Why choose SHH STEEL for GB/T 11251 Grade 30CrMnSi

  • We produce and export GB/T 11251-2025 Grade 30CrMnSi alloy structural steel plate
  • We review the enquiry for edition, grade, product route, delivery condition, dimensions and extra tests
  • We keep Table 1 annealed plate values distinct from high-temperature tempered hardness and from GB/T 3077 bar figures
  • We match documentation to what the purchase order requires

How to enquire for GB/T 11251 30CrMnSi plate

Item What to specify
Standard and grade GB/T 11251-2025 Grade 30CrMnSi
Product route Single-rolled plate, or continuous-rolled plate or strip
Delivery condition High-temperature tempered, annealed, normalized, normalized and tempered, quenched and tempered, or as-rolled for continuous-rolled material
Dimensions Required thickness, width and length; we confirm production and export feasibility against the enquiry
Chemistry Melt analysis to GB/T 3077, including any A or E quality class; request product analysis to GB/T 222 only if needed; state any agreed phosphorus or sulfur variant
Mechanical tests State whether Table 1 annealed values, hardness, normalized values or an agreed quenched-and-tempered package applies
Other tests Ultrasonic class if different from the standard Class II rule, bend testing for stamping, decarburization or inclusion rating only when written on the order
Documentation State the inspection document type required by the project

FAQ

Is GB/T 11251 30CrMnSi ordered only by chemistry?
Chemistry shall comply with GB/T 3077. For annealed single-rolled plate not thicker than 100 mm, Table 1 of GB/T 11251-2025 also sets tensile strength and elongation. High-temperature tempered plate is ordered to GB/T 3077 hardness. Other conditions are agreed on the contract.
Is 30CrMnSiA a separate Table 1 plate grade, and does Table 2 replace Table 1?
30CrMnSiA is the GB/T 3077 high-quality class of base grade 30CrMnSi, not an extra Table 1 row. Table 1 still covers annealed single-rolled plate. Table 2 is a specimen quench-and-temper test available only when clause 6.2.1.5 is agreed; those figures are not automatic as-delivered plate minima and are not GB/T 3077 bar values.
Does Table 1 apply to every delivery condition and thickness?
No. Table 1 applies to annealed single-rolled plate not thicker than 100 mm. Normalized plate keeps the Table 1 elongation and may use a tensile upper limit 50 MPa higher. Thickness over 100 mm, continuous-rolled tensile tests, and NT or QT supply are by agreement.
Did GB/T 11251-2025 replace GB/T 37601?
Yes. The 2025 edition replaces GB/T 11251-2020 and GB/T 37601-2019 and integrates the continuous-rolled content. Do not order this plate to the withdrawn 37601 specification as if it were still current.
What should a quotation enquiry include?
The ordered GB/T 11251 edition, Grade 30CrMnSi, single-rolled or continuous-rolled route, delivery condition, thickness by width by length, quantity, any extra chemical or mechanical tests, any NDE, and the inspection document required by the project.

Request a quotation

Contact SHH STEEL for a quotation for GB/T 11251-2025 Grade 30CrMnSi alloy steel plate. Please include your required quantity, plate thickness, width and length, whether you need single-rolled plate or continuous-rolled plate or strip, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the delivery condition. If your project requires tensile, hardness, toughness or ultrasonic testing beyond the standard rules, include the acceptance criteria and the inspection document required.

If you are considering 25CrMnSi, 35CrMnSi or the A quality class, or if you need the clause 6.2.1.5 specimen test, send the applicable standard and project specification with your enquiry. We will review the differences in product form, chemistry and supply condition rather than assume that related grades are interchangeable.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X