EN 10208-2 L245NB Steel Plate | Normalized Pipeline Plate
What is EN 10208-2 L245NB steel plate?
EN 10208-2 L245NB (steel number 1.0457) belongs to EN 10208-2 requirement class B with delivery condition NB (Normalized or normalizing formed). EN 10208 is a pipe standard for on-land combustible-fluid pipelines, primarily gas supply systems. Part 2 adds Charpy impact (Tables 6 or 7), tighter chemistry, yield-ratio control on the pipe product, and enhanced NDT versus Part 1.
EN 10208-1:2009 and EN 10208-2:2009 specify technical delivery conditions for steel PIPES for pipelines for combustible fluids (primarily on-land gas supply systems). They are not plate product standards. SHH supplies pipeline steel plate as feedstock for forming welded line pipe to the ordered EN 10208 grade chemistry and mechanical package; plate is not automatically certified as finished EN 10208 pipe. Confirm plate-as-feedstock scope, testing and documentation at quotation. Both EN 10208 parts were withdrawn/replaced in CEN catalogs by EN ISO 3183:2012 (later editions of EN ISO 3183 / ISO 3183 and API Spec 5L cover petroleum and natural gas industry line pipe). Historical gas-distribution RFQs may still cite EN 10208; match the project specification.
This page covers pipeline steel plate intended as feedstock for forming line pipe to the L245NB chemistry and mechanical package. Do not treat plate as certified finished EN 10208 pipe unless the order and MTC explicitly cover that scope.
Category hubs: Pipeline Steel Plates · EN 10208-2 · EN 10208-1 · API 5L.
Same delivery family: L290NB · L360NB · L415NB. Other EN 10208-2 grades: L290NB · L360NB · L415NB · L360QB · L415QB · L450QB · L485QB · L555QB · L245MB · L290MB · L360MB · L415MB · L450MB · L485MB · L555MB.
Material Specification for EN 10208-2 L245NB
| Parameter | Specification |
|---|---|
| Reference standard | EN 10208-2:2009 (withdrawn/replaced by EN ISO 3183 in CEN catalogs; confirm project edition) |
| Grade / number | L245NB / 1.0457 |
| Requirement class | B |
| Delivery condition | NB – Normalized or normalizing formed |
| Product form on this page | Pipeline steel plate for line-pipe forming (feedstock); confirm at quotation |
| Underlying EN product | Seamless and/or welded steel pipe per grade manufacturing table |
| Wall basis for tabulated values | T ≤ 25 mm in Tables 3 and 5; thicker by agreement up to 40 mm |
| SHH supply focus | About 6-50 mm plate (confirm against mill practice and order) |
| Width / length | About 1500-4000 mm width; length cut-to-size on request |
| Surface / edge | As-rolled or shot blasted; mill edge or cut edge |
| Certification | EN 10204 3.1 / 3.2 as ordered |
| Density | 7.85 g/cm³ |
Chemical Composition of EN 10208-2 L245NB (heat and product analysis)
Heat (cast) analysis limits for L245NB under EN 10208-2:2009 Table 3 (wall thickness T ≤ 25 mm). Product analysis shall not deviate from cast limits by more than Table 4. CEV = C + Mn/6 + (Cr+Mo+V)/5 + (Ni+Cu)/15 and is specified on the product analysis. Typical residual / deoxidation package (footnote e unless grade footnotes override): 0.015 ≤ Altot < 0.060; N ≤ 0.012; Al/N ≥ 2; Cu ≤ 0.25; Ni ≤ 0.30; Cr ≤ 0.30; Mo ≤ 0.10. For T > 25 mm up to 40 mm, chemistry is by agreement. Always verify the MTC.
| Element / index | Heat (cast) max / range |
|---|---|
| C | ≤0.16 |
| Si | ≤0.40 |
| Mn | ≤1.10 |
| P | ≤0.025 |
| S | ≤0.020 |
| V | – |
| Nb | – |
| Ti | – |
| CEV max (product analysis) | ≤0.42 |
Product-analysis plus tolerances (Table 4, selected): C +0.02 (≤0.21 cast); Si +0.05 (≤0.45); Mn +0.10 (≤1.80); P +0.005; S +0.005; V +0.01; Nb +0.01; Ti +0.01; Al ±0.005.
Elements not listed shall not be added intentionally without purchaser approval, except for deoxidation and heat finishing.
Mechanical Properties of EN 10208-2 L245NB
Tensile requirements for the pipe body under EN 10208-2:2009 Table 5 (T ≤ 25 mm). Yield is Rt0.5. Yield-to-tensile ratio Rt0.5/Rm applies to the product pipe and cannot be required of the starting plate alone; when ordering plate as feedstock, state whether pipe-body ratio control after forming is required. Elongation A is transverse; longitudinal values are 2 units higher. For T > 25 mm up to 40 mm, mechanics are by agreement.
| Grade | Rt0.5 (MPa) | Rm min (MPa) | Rt0.5/Rm max | A transverse min (%) | Bend mandrel |
|---|---|---|---|---|---|
| L245NB | 245-440 | ≥415 | ≤0.80 | ≥22 | 3T |
Impact (class B): Charpy V-notch at typically 0 °C; purchaser states Table 6 (safety factor 1.6) or Table 7 (safety factor 1.4). Energies are pipe-diameter and wall-thickness dependent. For D ≤ 510 mm many grades list transverse pipe-body average ≥40 J (individual ≥30 J) as the baseline cell; higher grades and larger diameters require higher values per Tables 6/7. DWT (drop-weight tear) by agreement for D > 500 mm, T > 8 mm and specified yield > 360 MPa. For plate feedstock, state intended pipe OD, wall and Table 6 vs 7 on the enquiry.
Hard spots / flattening: Any hard spot exceeding 50 mm in any direction shall have hardness < 35 HRC (327 HB) per EN 10208-2:2009 8.5.7 (cold-formed pipe surface). Not a sour-service hardness limit. Flattening test applies to HFW pipe production testing (EN ISO 8492), not to plate tensile coupons. Sour-service HIC/SSC or offshore packages are not defined inside EN 10208; specify ISO 3183 / API 5L Annex H/J or NACE/ISO 15156 when needed.
Density approximately 7.85 g/cm³.
Delivery Conditions for EN 10208-2 L245NB
NB means Normalized or normalizing formed. The delivery letter is built into the steel name L245NB.
NB: normalizing or normalizing forming. QB: quenching and tempering. MB: thermomechanical rolling (subsequent heating above about 580 °C may lower strength; TMCP properties generally cannot be restored by heat treatment alone).
For plate feedstock, order the plate delivery condition that matches the intended pipe route (Normalized or normalizing formed). State intended pipe type (S / HFW / SAW / COW) when it affects starting-material practice.
Weldability of EN 10208-2 L245NB
EN 10208-2 selects chemistry and CEV limits (where tabulated) so class B steels are weldable for pipe and pipeline fabrication. CEV for L245NB: ≤0.42. Welding behaviour still depends on consumables, procedure and joint restraint. Weldability data or weld tests may be agreed (option). Use a qualified WPS.
MB grades typically emphasize lower C / CEV for improved weldability relative to higher-C normalized routes at the same strength class. QB heats need care on heat input and HAZ toughness after Q&T.
Related: API 5L · API 5L Grade B / L245 (N) · EN 10208-1 class A.
Dimensional Tolerances for EN 10208-2 L245NB plate
EN 10208-2 dimensional tables cover finished pipe. For plate feedstock, use the agreed plate dimensional standard (for example EN 10029) unless the order cites another agreement. State flatness, edge condition, UT level and cut size when SAW/HFW forming tolerances are tight.
Applications and service limits for EN 10208-2 L245NB
Typical purchasing contexts for L245NB plate feedstock:
- On-land gas transmission / distribution projects citing EN 10208-2 class B with NB delivery
- Welded or seamless line-pipe forming requiring Charpy-controlled class B packages
- RFQs comparing L245NB with API 5L Grade B / L245 (N)
Not an automatic substitute for ISO 3183 / API 5L petroleum and natural gas industry line pipe. Not a dedicated sour or offshore annex; add those requirements explicitly when needed.
Related: Pipeline Steel Plates · EN 10208-2 · API 5L Grade B / L245 (N) · GB/T 21237 related.
Impact toughness package for EN 10208-2 L245NB
Charpy V-notch at typically 0 °C; purchaser states Table 6 (safety factor 1.6) or Table 7 (safety factor 1.4). Energies are pipe-diameter and wall-thickness dependent. For D ≤ 510 mm many grades list transverse pipe-body average ≥40 J (individual ≥30 J) as the baseline cell; higher grades and larger diameters require higher values per Tables 6/7. DWT (drop-weight tear) by agreement for D > 500 mm, T > 8 mm and specified yield > 360 MPa. For plate feedstock, state intended pipe OD, wall and Table 6 vs 7 on the enquiry.
On the plate enquiry, state: intended pipe outside diameter and wall, Table 6 vs Table 7, test temperature if not 0 °C, and whether DWT is required. Plate CVN orientation and sub-size rules should be agreed when full pipe transverse pieces are not available at plate stage.
Equivalent and related grades for EN 10208-2 L245NB
These grades are commonly compared with L245NB. They are approximate, not automatic substitutes.
| Standard / family | Grade | Relation | Product page |
|---|---|---|---|
| EN 10208-2 | L245NB | This page (NB) | – |
| API 5L / ISO 3183 | API 5L Grade B / L245 (N) | Approximate PSL2 talk | API 5L related |
| GB/T 21237 | Related PSL2 grade | Planned plate hub | GB/T 21237 |
| EN 10208-1 | GA class A | Lower requirement class; no mandatory Charpy | EN 10208-1 |
| Category | Pipeline hubs | Navigation | Pipeline Steel Plates · EN 10208-2 · API 5L |
EN 10208-2 L245NB vs related NB/QB/MB grades (selection aid)
Compare delivery routes and ratio/CEV caps at the same or related strength class. Not automatic substitutes.
| Grade | DC | Rt0.5 | Rm min | Ratio max | CEV | Page |
|---|---|---|---|---|---|---|
| L245NB | NB | 245-440 | ≥415 | ≤0.80 | ≤0.42 | This page |
| L245MB | MB | 245-440 | ≥415 | ≤0.85 | ≤0.40 | L245MB |
Why choose SHH STEEL for EN 10208-2 L245NB
- China mill-direct pipeline steel plate aligned to EN 10208-2 L245NB (Normalized or normalizing formed) for line-pipe forming
- EN 10204 3.1 mill test certificates; 3.2 and third-party inspection (SGS, TUV, BV) on request
- Clear feedstock wording: plate for forming to EN 10208 grade requirements, confirm at quotation
- Full NB / QB / MB coverage under EN 10208-2 · class A under EN 10208-1
- API 5L / GB/T 21237 talk when the project cites those standards: API 5L related · GB/T 21237
Supply, cutting and inspection for EN 10208-2 L245NB
| Item | SHH STEEL supply note |
|---|---|
| Thickness | About 6-50 mm focus; T > 25 mm chemistry/mechanics by agreement per standard |
| Size | Width about 1500-4000 mm; cut-to-size length on request |
| Delivery condition | NB – Normalized or normalizing formed |
| Processing | Cutting, beveling, shot blasting available |
| Mill certificate | EN 10204 3.1 standard; 3.2 on request |
| Third-party inspection | SGS, TUV, BV can be arranged |
| Quotation needs | Grade L245NB, thickness × width × length, quantity, CVN table (6 or 7) / OD / wall, UT level, inspection level |
FAQ
-
What does the NB suffix mean on L245NB?
- NB means Normalized or normalizing formed. It is part of the EN 10208-2 steel name.
-
Is L415NB a real EN 10208-2 grade?
- Yes. L415NB is steel number 1.8972 in EN 10208-2:2009 Table 1 (normalized or normalizing formed).
-
Is EN 10208-2 a plate standard?
- No. It is a pipe standard. This page covers pipeline steel plate for line-pipe forming to L245NB grade requirements; confirm at quotation.
-
What Charpy values apply?
- Diameter- and thickness-dependent per Tables 6 or 7 (typically at 0 °C). State pipe OD, wall and table choice on the enquiry.
-
Approximate API 5L talk?
- API 5L Grade B / L245 (N). See API 5L related. Substitution needs project approval.
Request a quotation
Send EN 10208-2 L245NB, thickness × width × length, quantity, Charpy table (6 or 7) with intended pipe OD/wall, any DWT/UT extras and inspection level. SHH STEEL will return mill availability, certification scope and a quotation for pipeline steel plate for line-pipe forming to EN 10208 grade requirements.
Contact: admin@steelspecs.com · +86-18939509537 · +86-021-62716097
More options: EN 10208-2 · Pipeline Steel Plates · API 5L · EN 10208-1