EN 10149-2 S700MC Steel Sheet and Plate
What is EN 10149-2 S700MC Steel Sheet and Plate?
EN 10149-2 S700MC Steel Sheet and Plate is a weldable, hot-rolled, high yield strength steel flat product for cold forming under EN 10149-2:2013, Hot rolled flat products made of high yield strength steels for cold forming — Part 2: Technical delivery conditions for thermomechanically rolled steels, used together with EN 10149-1:2013. The technical tables on this page follow EN 10149-2:2013 Table 1 (ladle analysis) and Table 2 (mechanical properties). That 2013 text lists eleven formal grades: S315MC, S355MC, S420MC, S460MC, S500MC, S550MC, S600MC, S650MC, S700MC, S900MC and S960MC. This page is S700MC (steel number 1.8974). S900MC and S960MC were added in 2013; they are not treated as if the list stopped at S700MC.
The products shall be supplied in the thermomechanically rolled delivery condition (clause 7.2). That is the “M” condition. It is not a normalized or normalized-rolled delivery (those steels belong to EN 10149-3). A note in clause 7.5.2.1 states that products supplied according to this standard are not suitable for hot forming.
EN 10149-2:2013 applies to hot-rolled flat products in stated thin thickness ranges: 1.5 mm to 20 mm for grades with a specified minimum yield strength from 315 MPa up to and including 460 MPa; 1.5 mm to 16 mm for 500 MPa up to and including 700 MPa; and 2 mm to 10 mm for 900 MPa to 960 MPa. For S700MC the applicable range is 1.5 mm to 16 mm. Those figures are the standard’s scope limits for this grade, not a thick-plate rolling-capacity guarantee.
The product form is hot-rolled flat steel: continuously hot-rolled strip and plate/sheet cut from wide strip (tolerances EN 10051) or hot-rolled plate (tolerances EN 10029, thickness class A unless otherwise agreed). SHH STEEL produces and exports EN 10149-2 S700MC Steel Sheet and Plate to the ordered thickness, tests and documentation. Related published ranges include High-Strength Low Alloy Plates and Structural Steel Plates.
Material specification for EN 10149-2 S700MC Steel Sheet and Plate
The items below follow EN 10149-2:2013 together with EN 10149-1:2013. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.
| Parameter | Detail |
|---|---|
| Standard | EN 10149-2:2013 (approved 17 August 2013; September 2013; supersedes EN 10149-2:1995), used with EN 10149-1:2013. Current listing on national catalogues checked for this draft. |
| Grade / number | S700MC / 1.8974 |
| Classification | Alloy special steel according to EN 10020 (clause 6.1) |
| Formal set | Eleven grades in Tables 1 and 2 and clause 6.1 (S315MC to S960MC). This page is S700MC |
| Product form | Hot-rolled flat products for cold forming: sheet/strip and thin plate within the scope thickness, not a thick-plate capacity claim |
| Scope thickness for this grade | 1.5 mm to 16 mm |
| Delivery condition | Thermomechanically rolled (clause 7.2) |
| Chemistry basis | EN 10149-2:2013 Table 1 ladle analysis. Product analysis is carried out if agreed (EN 10149-1 option 4); the purchaser specifies the number of samples and the elements to be determined. Permitted product-analysis deviations are those of EN 10149-1 for the edition named on the order and are not reprinted here. |
| Mechanical basis | EN 10149-2:2013 Table 2 (clause 7.4.1) |
| Carbon equivalent | Table 1 of this part does not specify a CEV or Ceq maximum. This page does not calculate one |
| Dimensional standards | EN 10029 class A thickness tolerances for hot-rolled plate unless otherwise agreed; EN 10051 for plate/sheet cut from strip |
| Our supply | We produce and export S700MC as sheet and plate to the thickness, tests and documentation agreed on the order |
Chemical composition of EN 10149-2 S700MC Steel Sheet and Plate
The chemical composition determined by ladle analysis shall comply with Table 1 of EN 10149-2:2013. The row below is the S700MC ladle-analysis row of that table. Table 1 does not specify a carbon-equivalent maximum, so no CEV or Ceq figure is calculated or printed here.
| Element | S700MC ladle analysis, EN 10149-2:2013 Table 1 (mass %) |
|---|---|
| C, max | 0.12 |
| Mn, max | 2.10 |
| Si, max | 0.60 |
| P, max | 0.025 |
| S, max | 0.015 (see note b) |
| Al total, min | 0.015 |
| Nb, max | 0.09 (see note a) |
| V, max | 0.20 (see note a) |
| Ti, max | 0.22 (see note a) |
| Mo, max | 0.50 |
| B, max | 0.005 |
Note a: the sum of Nb, V and Ti shall be max. 0.22 %. Note b: if agreed at the time of the order the sulphur content shall be max. 0.010 % (ladle analysis); see clause 11, option 12).
Product analysis is not automatic. EN 10149-1 option 4 applies when the purchaser agrees product analysis at enquiry and order and specifies the samples and elements. This page does not invent product-analysis deviation numbers beyond that rule.
Mechanical properties and thickness limits
Under the inspection conditions of clause 8 and the thermomechanically rolled delivery condition of clause 7.2, the mechanical properties shall comply with Table 2 of EN 10149-2:2013. The values below are that table for S700MC. Footnote d states that for thicknesses greater than 8 mm the minimum yield strength can be 20 MPa lower.
| Property | S700MC, EN 10149-2:2013 Table 2 |
|---|---|
| Minimum yield strength ReH | 700 MPa; for thicknesses > 8 mm this minimum can be 20 MPa lower (note d) |
| Tensile strength Rm | 750–950 MPa |
| Minimum elongation A, nominal thickness < 3 mm (L0 = 80 mm) | 10 % |
| Minimum elongation A, nominal thickness ≥ 3 mm (L0 = 5.65 √S0) | 12 % |
| Bending at 180°, minimum mandrel diameter | 2t |
| Scope thickness for this grade | 1.5 mm to 16 mm |
Note a: the values for the tensile test apply to longitudinal test pieces. Note b: the values for the bend test apply to transverse test pieces. Note c: t is the thickness in millimetres of the test piece for the bend test.
Impact energy is not a Table 2 requirement. Clause 7.4.2 states that if agreed at the time of the order, verification of the impact energy value shall be carried out in accordance with EN 10149-1 (option 5). If an impact test is agreed, clause 8.5.2 requires one sample sufficient for one set of six impact test pieces. This page does not invent a joule value or a test temperature.
Delivery conditions for EN 10149-2 S700MC Steel Sheet and Plate
EN 10149-2:2013 states:
- The products shall be supplied in the thermomechanically rolled delivery condition.
- The surface protection of descaled products shall be in accordance with EN 10149-1 (option 2).
- A note in clause 7.5.2.1 records that products supplied according to this standard are not suitable for hot forming.
- Recommendations regarding cold forming are laid down in CEN/TR 10347.
Do not treat normalized, normalized-rolled or quenched-and-tempered supply as the delivery condition of this part. EN 10149-3 covers the normalized or normalized-rolled “N” grades (S260NC, S315NC, S355NC and S420NC) and is a different specification.
We produce and export S700MC in the specified thermomechanically rolled condition, as sheet and plate within 1.5 mm to 16 mm.
Welding, coating and fabrication
Weldability shall be in accordance with EN 10149-1 (clause 7.5.1). This page does not invent preheat temperatures, heat-input limits or hardness caps. Table 1 of this part does not give a normative carbon-equivalent maximum, so no calculated CEV is offered as a welding index.
Clause 7.5.3 addresses hot-dip zinc coating for grades S315MC to S700MC: the chemical composition of steels to be hot-dip zinc coated shall be separately agreed. Option 7 of EN 10149-1 can be used to order a silicon and phosphorus composition in Category A, B or D of EN ISO 14713-2:2009, Table 1. The same clause notes that in some cases steels above S460 may be sensitive to cracking during galvanizing, so special care should be taken.
A procedure written only for EN 10025 structural plate, or only for quenched-and-tempered 690 MPa plate, is not automatically valid for thermomechanically rolled S700MC intended for cold forming.
Form, finish and dimensions
Dimensions and tolerances shall be in accordance with EN 10149-1. For hot-rolled plate, the basic requirements shall be in accordance with EN 10029, including thickness tolerances to class A, unless otherwise agreed at the time of the order. For plates cut from continuously hot-rolled strip, thickness tolerances shall be in accordance with EN 10051. This page does not reprint those tolerance tables and does not list stock sizes or mill-capacity ranges.
We produce and export S700MC to the dimensions and surface requirements agreed on the enquiry, within the standard’s thin flat-product scope.
Applications and specification limits
S700MC is specified for cold-formed parts that name EN 10149-2 and this grade, including formed members, brackets and similar thin hot-rolled flat products that need the stated yield class and improved formability. The products are suitable for flanging without cracking (clause 7.5.2.2.2). Suitability for roll forming follows EN 10149-1 (option 6). Allowable design stresses and any toughness rule come from the construction code or purchaser specification, not from Table 2 alone.
Table 2 specifies a 180° bend test on transverse test pieces, with a minimum mandrel diameter of 2t. Annex B is informative. It recommends minimum inside bend radii for cold forming at bend angles of 90° or less: 1.5t for t ≤ 3 mm, 2.0t for 3 mm < t ≤ 6 mm, and 2.5t for t > 6 mm. Those Annex B figures are recommendations, not Table 2 requirements.
This page is not EN 10025-2 structural plate, not EN 10025-6 quenched-and-tempered plate, and not EN 10149-3 normalized plate. The standard limits S700MC to 1.5 mm to 16 mm.
Compare EN 10149-2 S700MC Steel Sheet and Plate with other steel products
EN 10149-2 S700MC Steel Sheet and Plate is thermomechanically rolled flat steel for cold forming under EN 10149-2, not normalized EN 10149-3 plate and not quenched-and-tempered high-strength plate. The comparison uses three products we already publish. They are related by engineering use or similar names, not equivalents. Unpublished EN 10149-2 sibling grades are not linked here.
| Material | Alloy / type | Delivery condition | Mechanical requirements | Typical service | Substitution limit |
|---|---|---|---|---|---|
| EN 10149-2 S700MC Steel Sheet and Plate (this product) | EN 10149-2:2013 S700MC (1.8974); ladle analysis to Table 1; alloy special steel | Thermomechanically rolled; not suitable for hot forming | Table 2: ReH min 700 MPa; Rm 750–950 MPa; A 10 % (L0 = 80 mm, < 3 mm) / 12 % (L0 = 5.65 √S0, ≥ 3 mm); 180° bend mandrel 2t; thickness 1.5 mm to 16 mm | Cold-formed thin hot-rolled sheet and plate specified to EN 10149-2 S700MC | Not interchangeable with EN 10025 structural or QT names unless the project specification allows it |
| EN 10025-2 S355JR Steel Plate | From our S355JR page: EN 10025-2 structural steel | From our S355JR page: high-strength structural steel plate | From our S355JR page: 355 MPa yield strength | General structural plate specified to EN 10025-2 S355JR | Not an equivalent. S355JR is not the EN 10149-2 thermomechanical cold-forming system, and its usual thickness range is not the thin flat-product scope of S700MC |
| EN 10025-2 S355J2 Steel Plate | From our S355J2 page: EN 10025-2 structural steel | From our S355J2 page: high-strength structural steel plate | From our S355J2 page: 355 MPa yield strength and −20 °C impact toughness | Structural plate specified to EN 10025-2 S355J2 | Not an equivalent. Impact at −20 °C is part of the J2 designation on that page; EN 10149-2 impact verification is optional (option 5) and is not a Table 2 value |
| EN 10025-6 S690QL Steel Plate | From our S690QL page: EN 10025-6 quenched-and-tempered structural steel | From our S690QL page: quenched and tempered | From our S690QL page: 690 MPa yield strength with toughness at −40 °C | High-strength QT structural plate specified to S690QL | Different heat treatment, a different toughness rule and a different thickness practice. Not a substitute stamp for thermomechanically rolled S700MC |
Related published ranges: High-Strength Low Alloy Plates and Structural Steel Plates.
Equivalent and related grades by country
The designations below are near names or related national plates, not certified or automatic equivalents. Chemistry, thickness, delivery condition, bend rules and the required stamp must match the project specification before a substitution is considered. Unpublished EN 10149-2 siblings are named as plain text only.
| Country / region | Standard | Grade | Similarity and key differences | Substitution caveat |
|---|---|---|---|---|
| Europe | EN 10149-2:2013 | S700MC | This thermomechanically rolled flat product for cold forming. The formal list is S315MC, S355MC, S420MC, S460MC, S500MC, S550MC, S600MC, S650MC, S700MC, S900MC and S960MC. | Specify EN 10149-2, this named grade, thickness within 1.5 mm to 16 mm, the thermomechanically rolled condition and any options (including option 5 or 12). |
| Europe | EN 10149-3 | S260NC, S315NC, S355NC or S420NC as applicable | Normalized or normalized-rolled cold-forming steels in Part 3, not the “M” condition of Part 2. | Do not treat an NC name as an automatic MC match. |
| Europe | EN 10025-2 | S355JR or S355J2 | From our live pages: S355JR has a 355 MPa yield; S355J2 has a 355 MPa yield and −20 °C impact toughness. | Different family. See EN 10025-2 S355JR Steel Plate and EN 10025-2 S355J2 Steel Plate. |
| Europe | EN 10025-6 | S690QL | From our S690QL page: quenched-and-tempered plate, 690 MPa yield, toughness at −40 °C. | Different family. See EN 10025-6 S690QL Steel Plate. |
| China | GB/T 1591 | Q690M names used in catalogues | Chinese HSLA / TMCP plates written to GB/T 1591, not to EN 10149-2. From our Q355MC page: 355 MPa yield and 0 °C impact, and that page is not hot-rolled Q355C or normalized Q355NC. From our Q355B page: 355 MPa yield and +20 °C impact. | Do not assume a Q-number, even Q355MC, is an automatic S355MC equivalent. See Q355MC TMCP Steel Plate and Q355B Steel Plate. |
| United States | ASTM A572/A572M | Grade 50 | From our A572 Grade 50 page: yield 345 MPa (50 ksi) min and tensile 450 MPa (65 ksi) min, usually hot-rolled or controlled-rolled. | Not the EN 10149-2 type system. See ASTM A572 Grade 50 Structural Steel Plate. |
Why choose SHH STEEL for EN 10149-2 S700MC Steel Sheet and Plate
- We produce and export EN 10149-2 S700MC thermomechanically rolled sheet and plate for cold forming
- We review the enquiry for edition, grade, thickness within 1.5 mm to 16 mm, and options
- We keep the M delivery condition distinct from normalized EN 10149-3 and from quenched-and-tempered plate
- We do not treat impact testing as automatic, and we do not invent a CEV where Table 1 gives none
- We match documentation to what the purchase order requires
How to enquire for EN 10149-2 S700MC Steel Sheet and Plate
| Item | What to specify |
|---|---|
| Standard and grade | EN 10149-2, S700MC (1.8974). Name the edition required by the project. Figures on this page follow EN 10149-2:2013 |
| Product form | Hot-rolled flat product: sheet, strip or thin plate. State which form is required |
| Thickness and dimensions | Thickness, width and length. The standard limits S700MC to 1.5 mm to 16 mm |
| Delivery condition | Thermomechanically rolled (M); not normalized |
| Chemistry | Table 1 ladle analysis, including note a (Nb + V + Ti max. 0.22 %) and, if required, option 12 for sulphur max. 0.010 %. Write product analysis only if option 4 is required |
| Mechanical tests | Table 2 tension (longitudinal) and 180° bend (transverse). Write option 5 if impact verification is required; it is not automatic |
| Coating / forming extras | Option 7 if a galvanizing composition category is required; option 6 if roll-forming suitability must be agreed |
| Documentation | State the inspection document type required by the project |
| Processing | Cutting or other processing only when requested |
Request a quotation
Contact SHH STEEL for a quotation for EN 10149-2 S700MC thermomechanically rolled sheet and plate for cold forming. Please include your required quantity, thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.
Specify EN 10149-2, S700MC (1.8974), and the edition required by the project. Figures on this page follow EN 10149-2:2013. The standard limits this grade to 1.5 mm to 16 mm. Write option 5 if impact verification is required; it is not automatic.
If your enquiry compares S700MC with EN 10025-2 S355JR, EN 10025-2 S355J2 or EN 10025-6 S690QL, identify each product clearly. We will review the differences in standard, delivery condition, thickness scope and toughness rules rather than assume that similar yield numbers are interchangeable.
For a detailed quotation, email your material specification, quantity and delivery requirements to our team.
Contact: admin@steelspecs.com