EN 10025-4 S355ML H-beam is a thermomechanically rolled European H-section with 355 MPa minimum yield in the first thickness band and a 27 J impact requirement at −50 °C. The page also lists S355M, HEA, HEB and IPE sizes, and the long-product carbon and thickness footnotes that apply to sections.
Keywords
EN 10025-4 S355ML H-Beam, S355ML H-beam, S355M, 1.8834, HEA HEB IPE
Equivalent Grades:
S355M (same standard, −20 °C quality); S355J2; S355JR; Q355B; SM490 — comparisons only, not automatic substitutes.
Share:
General Description
Material Specification
Available Sizes of S355ML H-Beam
Chemical Composition of S355ML H-Beam
Carbon Equivalent of S355ML H-Beam
Mechanical Properties of S355ML H-Beam
Delivery Conditions, Inspection and Identification
Weldability of S355ML H-Beams
Shape Tolerances and Theoretical Mass
Applications and Service Limits
S355ML Compared with S355M, S355J2 and Q355B
Near-Equivalents: Not Automatic Substitutes
Sourcing S355ML H-Beams from SHH STEEL
FAQ
Conclusion

What is EN 10025-4 S355ML H-Beam?

EN 10025-4 S355ML H-beam is a hot-rolled European H-section in thermomechanically rolled weldable fine-grain structural steel S355ML (steel number 1.8834). The material standard is EN 10025-4. Dimensions and theoretical masses for the HEA, HEB and IPE series on this page are those of EN 10365. Shape and dimensional tolerances for I and H sections are those of EN 10034. S marks a structural steel, 355 is the minimum yield strength in MPa up to 16 mm, M is the thermomechanical delivery condition, and L is the quality with a longitudinal Charpy V-notch requirement of 27 J at −50 °C when impact testing applies.

The related M quality, S355M (1.8823), is listed on this page for comparison. It shares the tensile table and the CEV table, but its standard impact verification is 40 J at −20 °C, not the ML −50 °C test. These beams are filed under steel beam profiles in the steel structural profiles category. They are not as-rolled EN 10025-2 sections, and they are not GB/T 11263 HW, HM or HN sections of a similar depth.

Material, Dimensions and the M / ML Quality Family

The purchase order and the inspection document should name, separately:

  • EN 10025-4 and its edition (this page uses the 2004 edition as the numeric basis; the edition named on the order governs), the grade S355ML or S355M, and the delivery condition M;
  • the EN 10365 designation (for example HE 200 A, HE 200 B or IPE 300) and the edition used for dimensions and mass;
  • the carbon equivalent, the required impact test (including a transverse Table 7 test only if it is agreed), and the inspection document type.

S355ML is a thermomechanically rolled fine-grain steel. It is not an as-rolled EN 10025-2 grade and is not a normalized EN 10025-3 grade.

S355ML H-Beam Sizes: EN 10365 HEA, HEB and IPE Series

The tables are the same verified EN 10365:2017 HEA, HEB and IPE series used on the S355JR H-beam page: 24 HEA sizes from HE 100 A to HE 1000 A, 24 HEB sizes from HE 100 B to HE 1000 B, and 18 IPE sizes from IPE 80 to IPE 600. EN 10365:2017 is the numeric basis. EN 10365:2026 is a later dimensional edition; official 2026 tables are not used on this page. The edition named on the order governs. Universal beams and universal columns can be reviewed when they are named on the enquiry; they are not tabulated here. Not every mill rolls every designation in S355ML.

HEA series

Swipe horizontally to view all dimensions.

Designation h (mm) b (mm) tw (mm) tf (mm) r (mm) A (cm²) Mass (kg/m)
HE 100 A 96 100 5 8 12 21.2 16.7
HE 120 A 114 120 5 8 12 25.3 19.9
HE 140 A 133 140 5.5 8.5 12 31.4 24.7
HE 160 A 152 160 6 9 15 38.8 30.4
HE 180 A 171 180 6 9.5 15 45.3 35.5
HE 200 A 190 200 6.5 10 18 53.8 42.3
HE 220 A 210 220 7 11 18 64.3 50.5
HE 240 A 230 240 7.5 12 21 76.8 60.3
HE 260 A 250 260 7.5 12.5 24 86.8 68.2
HE 280 A 270 280 8 13 24 97.3 76.4
HE 300 A 290 300 8.5 14 27 112.5 88.3
HE 320 A 310 300 9 15.5 27 124.4 97.6
HE 340 A 330 300 9.5 16.5 27 133.5 105
HE 360 A 350 300 10 17.5 27 142.8 112
HE 400 A 390 300 11 19 27 159.0 125
HE 450 A 440 300 11.5 21 27 178.0 140
HE 500 A 490 300 12 23 27 197.5 155
HE 550 A 540 300 12.5 24 27 211.8 166
HE 600 A 590 300 13 25 27 226.5 178
HE 650 A 640 300 13.5 26 27 241.6 190
HE 700 A 690 300 14.5 27 27 260.5 204
HE 800 A 790 300 15 28 30 285.8 224
HE 900 A 890 300 16 30 30 320.5 252
HE 1000 A 990 300 16.5 31 30 346.8 272

HEB series

Swipe horizontally to view all dimensions.

Designation h (mm) b (mm) tw (mm) tf (mm) r (mm) A (cm²) Mass (kg/m)
HE 100 B 100 100 6 10 12 26.0 20.4
HE 120 B 120 120 6.5 11 12 34.0 26.7
HE 140 B 140 140 7 12 12 43.0 33.7
HE 160 B 160 160 8 13 15 54.3 42.6
HE 180 B 180 180 8.5 14 15 65.3 51.2
HE 200 B 200 200 9 15 18 78.1 61.3
HE 220 B 220 220 9.5 16 18 91.0 71.5
HE 240 B 240 240 10 17 21 106.0 83.2
HE 260 B 260 260 10 17.5 24 118.4 93.0
HE 280 B 280 280 10.5 18 24 131.4 103
HE 300 B 300 300 11 19 27 149.1 117
HE 320 B 320 300 11.5 20.5 27 161.3 127
HE 340 B 340 300 12 21.5 27 170.9 134
HE 360 B 360 300 12.5 22.5 27 180.6 142
HE 400 B 400 300 13.5 24 27 197.8 155
HE 450 B 450 300 14 26 27 218.0 171
HE 500 B 500 300 14.5 28 27 238.6 187
HE 550 B 550 300 15 29 27 254.1 199
HE 600 B 600 300 15.5 30 27 270.0 212
HE 650 B 650 300 16 31 27 286.3 225
HE 700 B 700 300 17 32 27 306.4 241
HE 800 B 800 300 17.5 33 30 334.2 262
HE 900 B 900 300 18.5 35 30 371.3 291
HE 1000 B 1000 300 19 36 30 400.0 314

IPE series

Swipe horizontally to view all dimensions.

Designation h (mm) b (mm) tw (mm) tf (mm) r (mm) A (cm²) Mass (kg/m)
IPE 80 80.0 46.0 3.8 5.2 5 7.6 6.0
IPE 100 100.0 55.0 4.1 5.7 7 10.3 8.1
IPE 120 120.0 64.0 4.4 6.3 7 13.2 10.4
IPE 140 140.0 73.0 4.7 6.9 7 16.4 12.9
IPE 160 160.0 82.0 5.0 7.4 9 20.1 15.8
IPE 180 180.0 91.0 5.3 8.0 9 23.9 18.8
IPE 200 200.0 100.0 5.6 8.5 12 28.5 22.4
IPE 220 220.0 110.0 5.9 9.2 12 33.4 26.2
IPE 240 240.0 120.0 6.2 9.8 15 39.1 30.7
IPE 270 270.0 135.0 6.6 10.2 15 45.9 36.1
IPE 300 300.0 150.0 7.1 10.7 15 53.8 42.2
IPE 330 330.0 160.0 7.5 11.5 18 62.6 49.1
IPE 360 360.0 170.0 8.0 12.7 18 72.7 57.1
IPE 400 400.0 180.0 8.6 13.5 21 84.5 66.3
IPE 450 450.0 190.0 9.4 14.6 21 98.8 77.6
IPE 500 500.0 200.0 10.2 16.0 21 115.5 90.7
IPE 550 550.0 210.0 11.1 17.2 24 134.4 106
IPE 600 600.0 220.0 12.0 19.0 24 156.0 122

S355ML Chemical Composition (Ladle and Product Analysis)

The figures below are from EN 10025-4:2004 Tables 2 and 3 for S355ML. For these H-sections the long-product footnotes apply: the ladle carbon maximum is 0.16%, the product-analysis carbon maximum is 0.18%, and phosphorus and sulphur maxima may be 0.005% higher than the tabulated flat-product figures. The aluminium minimum does not apply if sufficient other nitrogen-binding elements are present. Copper above 0.40% on the ladle analysis (0.45% on the product analysis) may cause hot shortness during hot forming.

Element Ladle analysis, S355ML (mass %) Product analysis, S355ML (mass %)
C max 0.14 (0.16 for long products) 0.16 (0.18 for long products)
Si max 0.50 0.55
Mn max 1.60 1.70
P max 0.025 (0.030 for long products) 0.030 (0.035 for long products)
S max 0.020 (0.025 for long products) 0.025 (0.030 for long products)
Nb max 0.05 0.06
V max 0.10 0.12
Al total, min 0.02 0.015
Ti max 0.05 0.06
Cr max 0.30 0.35
Ni max 0.50 0.55
Mo max 0.10 0.13
Cu max 0.55 0.60
N max 0.015 0.017

S355ML Carbon Equivalent

Table 4 of EN 10025-4:2004 gives the following CEV maxima, based on the ladle analysis, for S355M and S355ML. For long products the last column applies up to 150 mm. CEV is calculated by the IIW formula in the standard.

Nominal thickness (mm) Maximum CEV (%)
t ≤ 16 0.39
16 < t ≤ 40 0.39
40 < t ≤ 63 0.40
63 < t ≤ 120 0.45
120 < t ≤ 150 (long products) 0.45

S355ML Mechanical Properties: Yield, Tensile and −50 °C Impact

Tensile properties follow Table 5 of EN 10025-4:2004. Thickness is that of the part from which the test sample is taken, ordinarily the flange for these H-sections. For all products other than wide plate and strip, the tensile direction is parallel to the rolling direction. Footnote d of Table 5 extends the last thickness column to 150 mm for long products; those are the figures shown in the last row.

Nominal thickness (mm) Min. yield ReH (MPa) Tensile strength Rm (MPa) Min. elongation A (%)
t ≤ 16 355 470–630 (t ≤ 40) 22
16 < t ≤ 40 345 470–630 22
40 < t ≤ 63 335 450–610 22
63 < t ≤ 80 325 440–600 22
80 < t ≤ 100 325 440–600 22
100 < t ≤ 150 (long products) 320 430–590 22

When impact testing applies, Table 6 (longitudinal) and, only when agreed, Table 7 (transverse) give the following values, in joules:

Swipe horizontally to view all dimensions.

Quality Direction +20 °C 0 °C −10 °C −20 °C −30 °C −40 °C −50 °C
S355ML Longitudinal 63 55 51 47 40 31 27
S355M Longitudinal 55 47 43 40 — — —
S355ML (when agreed) Transverse 40 34 30 27 23 20 16

The usual verification test for S355ML is 27 J at −50 °C, longitudinal. S355M is verified at 40 J at −20 °C and has no standard Table 6 values below −20 °C. An S355M certificate does not demonstrate the ML −50 °C test. A lower test temperature, or a transverse Table 7 test, should be written on the order if it is required.

Delivery Conditions, Inspection and Identification

S355ML and S355M are supplied in the thermomechanical delivery condition M. The inspection document should identify EN 10025-4 and its edition, the grade S355ML or S355M and steel number, the delivery condition, the carbon equivalent, the EN 10365 designation and the edition used for dimensions and mass, ladle analysis, and tensile and impact results against the thickness at the test location, ordinarily the flange. A plate certificate, or an EN 10025-2 S355J2 certificate, does not, by itself, identify an S355ML H-beam.

Weldability of S355ML H-Beams

S355ML is specified as a weldable fine-grain structural steel. Preheat and consumable choice should use the certified heat analysis, the certified CEV, the actual flange thickness and the joint design. A long-product carbon or phosphorus-and-sulphur footnote used on the heat should appear on the certificate.

EN 10365 and EN 10034 Shape Tolerances and Theoretical Mass

Dimensions and theoretical masses belong to the ordered edition of EN 10365. Shape and dimensional tolerances for these I and H sections belong to EN 10034, not to EN 10279. Millimetre tolerance tables are not reproduced here. Settlement on theoretical or weighed mass should follow the contract and the named edition.

Applications and Service Limits

S355ML H-beams are used in welded structures where a thermomechanically rolled 355 MPa European section with a −50 °C impact quality is named. They are not a silent substitute for EN 10025-2 S355J2 H-beam, for EN 10025-2 S355JR H-beam, or for a Chinese or Japanese H-section of similar depth. S355M may be considered only when the −20 °C M quality is the one actually specified.

S355ML Compared with S355M, S355J2 and Q355B

The comparisons below are an orientation only; they are not automatic substitutes.

Grade / designation Standard Relationship to S355ML H-beam Caution
S355M EN 10025-4; same EN 10365 series The related M quality on this page, verified at −20 °C (40 J longitudinal) rather than −50 °C. M is not ML. Do not treat an S355M certificate as an S355ML result.
S355J2 / S355JR EN 10025-2; dimensions EN 10365 Non-alloy structural comparisons in the same 355 MPa class, usually as-rolled. J2 is −20 °C / 27 J, not the ML −50 °C table, and the delivery condition is not TM. See EN 10025-2 S355J2 H-beam.
Q355D / Q355B GB/T 1591; dimensions GB/T 11263 Chinese 355 MPa comparisons on the HW/HM/HN series. An HW is not an HEA. See GB/T 11263 Q355B H-beam.
SM490 JIS G 3106; dimensions JIS G 3192 A Japanese welded-structure comparison in the 490 N/mm² tensile class. A JIS H designation is not an EN 10365 section. See JIS G 3106 SM490 H-beam.

Near-Equivalents: Not Automatic Substitutes

A near-equivalent is a starting point for a discussion, not a licence to swap certificates. If a project names S355ML, keep that grade, the thermomechanical condition and EN 10365 on the order. The as-rolled European sisters are EN 10025-2 S355J2 H-beam and EN 10025-2 S355JR H-beam.

Sourcing S355ML H-Beams from SHH STEEL

SHH STEEL supplies EN 10025-4 S355ML H-beams against a named designation list, the quality (ML or M), the material edition and the inspection document type. Enquiries should state the HEA, HEB or IPE designations, whether a transverse impact test is required, cut lengths or mill lengths, any processing, and whether EN 10025-2 S355J2 H-beam is acceptable on part of the list.

The size table is the standard HEA, HEB and IPE series, not a claim that every designation is rolled in S355ML. Once the list is clear, a quotation can be prepared against the stated edition and certificate.

S355ML H-Beam FAQs

Is S355ML the same as S355M or S355J2?
No. S355ML and S355M share the EN 10025-4 tensile and CEV tables, but ML is verified at 27 J at −50 °C and M at 40 J at −20 °C. S355J2 is an EN 10025-2 as-rolled grade, verified at 27 J at −20 °C, and is not a thermomechanical ML steel.
Which carbon maximum applies to an S355ML H-beam?
For long products, Table 2 footnote e raises the ladle carbon maximum for S355 to 0.16%, and Table 3 footnote e raises the product-analysis maximum to 0.18%. The 0.14% and 0.16% flat-product figures are not the long-product limits.
Do the last yield and CEV bands stop at 120 mm on a section?
No. Table 5 footnote d states that for long products a thickness of 150 mm or less applies, so the last yield, tensile and CEV column is used up to 150 mm for these H-sections.
Which edition of EN 10025-4 is used on this page?
The numeric tables use EN 10025-4:2004. A later edition may be named on the order; the ordered edition governs.

Request a Quotation for EN 10025-4 S355ML H-Beam

EN 10025-4 S355ML H-beam is a thermomechanically rolled European H-section with 355 MPa minimum yield in the first thickness band and a 27 J impact requirement at −50 °C. Nominate the EN 10365 designation (for example HE 200 A or IPE 300), the quality (S355ML or S355M), EN 10025-4:2004 or the edition on the order, and the inspection document type. Send the size list, quality, edition, certificate type and any processing notes; SHH STEEL will review the package and quote accordingly.

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response