BS 1501 225 Grade 490B Steel Plate | BS 1501 Steel - SHH STEEL

BS 1501 225 Grade 490B Steel Plate

BS 1501-225 Grade 490B is a fully killed, niobium- and aluminium-treated carbon-manganese steel plate for pressure vessels. Heat-analysis carbon is 0.20 % maximum and manganese is 0.90–1.60 %. Yield strength is 355 N/mm² minimum up to 16 mm, and tensile strength is 490–610 N/mm². Suffix B adds characteristic elevated-temperature proof-stress values to those room-temperature tensile properties. Delivery is normalized unless another condition is agreed. SHH STEEL produces and exports 225 Grade 490B plate to the ordered edition, condition and dimensions.
Equivalent Grades:
EN 10028-3 P355NH is a later fine-grain vessel name (near name only).
Heat Treatment
Normalized, unless an alternative condition is agreed.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is BS 1501-225 Grade 490B plate?

We produce and export BS 1501-225 Grade 490B as fully killed, niobium- and aluminium-treated carbon-manganese steel plate for fired and unfired pressure equipment. Typical service includes welded boilers, vessels and similar parts that specify type 225 grade 490B.

BS 1501-1:1980 lists eight steel types, each with one or more tensile grades and, where Table 1 allows, suffix A or B and optional impact suffixes. This page specifies only 225 Grade 490B. It is not type 223 or 224, and it is not a BS 1501-2 alloy or BS 1501-3 stainless plate. Suffix A specifies room-temperature tensile properties only. LT20, LT30, LT50 and the L nickel limit are ordering options, not separate grades.

Composition and room-temperature tensile properties on this page follow BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates, the last final edition of Part 1. BS 1501-1:1980 was published on 28 November 1980 and withdrawn on 15 February 1993. It replaced BS 1501: Part 1: 1964 and that edition’s addenda. It was replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Those successor designations are not automatic aliases for the 1980 type-and-grade names. Name the edition or successor standard required on the purchase order.

The chemical and tensile figures below follow BS 1501-1:1980 as tabulated for this designation, including a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 values. BS 1501-2 (alloy plates) and BS 1501-3 (corrosion- and heat-resisting plates, sheet and strip) are different parts of the same historical series.

SHH STEEL produces and exports BS 1501-225 Grade 490B plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for BS 1501-225 Grade 490B

The items below follow BS 1501-1:1980. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard BS 1501-1:1980, Steels for pressure purposes — Specification for carbon and carbon manganese steels: plates
Official designation BS 1501-225 Grade 490B
Steel type Fully killed niobium- and aluminium-treated carbon-manganese steel
Product form Hot-rolled steel plate (this part does not cover bars, sections, forgings, tubes or stainless sheet)
How designations are listed Type number, tensile grade and suffix A or B; optional LT or RT impact suffixes where Table 1 allows; optional L after types 223, 224 and 225 when nickel is limited to 0.30 %
Applicable thickness Up to and including 150 mm
Usual heat treatment Normalized, unless an alternative condition is agreed.
Chemical analysis Ladle analysis as tabulated for this type and grade in BS 1501-1:1980
Tensile properties Yield strength, tensile strength and elongation, by thickness, from that edition
Our supply We produce and export 225 Grade 490B plate to the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of BS 1501-225 Grade 490B

The figures below are ladle analysis for BS 1501-225 Grade 490B from BS 1501-1:1980. Values are in weight percent and follow BS 1501-1:1980, including a reprint incorporating Amendments No. 1 to No. 3. They are not current EN 10028 values.

Element 225 Grade 490B ladle analysis, BS 1501-1:1980 (wt. %)
Carbon (C) 0.20 max
Silicon (Si) 0.10–0.50
Manganese (Mn) 0.90–1.60
Phosphorus (P) 0.030 max
Sulfur (S) 0.030 max
Aluminium (Al), metallic 0.015 min
Niobium (Nb) 0.010–0.060
Chromium (Cr) 0.25 max
Copper (Cu) 0.30 max
Molybdenum (Mo) 0.10 max
Nickel (Ni) 0.75 max

Figures are ladle analysis as tabulated for type 225 grade 490 in BS 1501-1:1980. Determination of total aluminium is deemed to meet the metallic aluminium requirement if the value obtained is not less than 0.018 %. The general residual nickel limit follows the same rule as types 223 and 224 (0.75 % maximum), with a combined total of chromium, copper and molybdenum of 0.50 % maximum. The optional L suffix after the type number limits nickel to 0.30 % and then limits chromium + copper + molybdenum + nickel to 0.70 %. L is an ordering option, not a separate product page. Project acceptance of the chemical analysis should be agreed against the named edition.

Elevated-temperature numerical values for suffix B belong in Appendix E and should be taken from the edition named on the order.

Tensile and related properties for BS 1501-225 Grade 490B

225 Grade 490B has thickness-dependent yield strength, tensile strength and elongation. Values below are from BS 1501-1:1980, including a reprint incorporating Amendments No. 1 to No. 3, and are not current EN 10028 values. Strength values are in N/mm², equivalent to MPa.

Thickness Tensile strength Rm, N/mm² Yield strength Re, N/mm² min Elongation A, % min
Over 3 mm up to and including 16 mm 490–610 355 21
Over 16 mm up to and including 40 mm 490–610 345 21
Over 40 mm up to and including 63 mm 490–610 340 20
Over 63 mm up to and including 100 mm 490–610 Reduced by the 1 % per 5 mm rule 20
Over 100 mm up to and including 150 mm 490–610 Reduced by the 1 % per 5 mm rule 20

The tensile window is that stated for type 225 grade 490 in BS 1501-1:1980 (490–610 N/mm²). Type 225 covers plates up to and including 150 mm. For plates over 63 mm up to and including 150 mm, yield strength is the 40 mm to 63 mm value reduced by 1 % for each 5 mm or part thereof increase in thickness. Table 1 lists optional impact suffixes LT20, LT30 and LT50 for this grade; those are ordering options, not separate product pages. If impact tests are specified, the acceptance values shall be taken from the named edition. Project acceptance of the tensile figures should be agreed against the named edition.

Suffix B specifies characteristic elevated-temperature yield or 0.2 % proof-stress values in Appendix E. Those high-temperature figures should be taken from the edition named on the order.

Delivery conditions for BS 1501-225 Grade 490B

Type 225 is supplied as fully killed, niobium- and aluminium-treated carbon-manganese steel plate. The 1980 text specifies supply in the normalized condition, unless an alternative condition of supply is agreed. Controlled rolling may be agreed under the general supply clause that applies to types 223 and 225. Name the required delivery condition on the purchase order.

If the project has moved to EN 10028-2 or EN 10028-3, order the successor designation and edition expressly. A later name is not by itself a substitute instruction.

The purchase order should name the official designation including the A or B suffix, any required impact suffix, thickness, width and length, the delivery condition, any extra tests, and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

BS 1501-1:1980 does not set a welding procedure. Type 225 is a fully killed, niobium- and aluminium-treated carbon-manganese vessel plate intended for welded pressure equipment. Welding and thermal cutting should be qualified for the carbon content, thickness and delivery condition.

Heat input and any required post-weld heat treatment belong in the project specification.

Form, appearance, dimensions and thickness tolerances

Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate tolerances when that standard is specified.

Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.

Applications and specification limits

We produce and export 225 Grade 490B plate as fully killed, niobium- and aluminium-treated carbon-manganese steel plate for fired and unfired pressure equipment. Typical service includes welded boilers, vessels and similar parts that specify type 225 grade 490B. The 1980 type 225 clauses cover this niobium- and aluminium-treated carbon-manganese plate. This page specifies grade 490 only.

BS 1501-1:1980 is a historical carbon and carbon-manganese plate standard for pressure purposes. It is not the current EN 10028-2 or EN 10028-3 order unless that successor standard is written on the enquiry, and it is not a BS 1501-2 alloy, BS 1501-3 stainless, BS 1502 bar or BS 1503 forging order.

Compare BS 1501-225 Grade 490B with other steel plates

225 Grade 490B is a BS 1501-1:1980 pressure-vessel plate. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
BS 1501-225 Grade 490B (this plate) BS 1501-1:1980 official designation Normalized, unless an alternative condition is agreed. Yield 355 N/mm² minimum up to 16 mm; tensile 490–610 N/mm², with suffix B elevated-temperature properties Typical service includes welded boilers and vessels that specify type 225 grade 490B A different standard, later EN name, or 1980 type is not an automatic substitute
EN 10028-3 P355NH Weldable fine-grain elevated-temperature vessel plate, steel number 1.0565 As specified in EN 10028-3 Published yield 355 MPa and tensile 490–630 MPa Modern European fine-grain boiler and vessel plate Related strength class only; chemistry and impact rules follow EN 10028-3
GB/T 713 Q345R Later Chinese carbon-manganese vessel plate As specified in GB/T 713 Published yield 345 MPa and tensile 510–640 MPa Modern Chinese boiler and vessel plate Related strength class only
EN 10028-2 P355GH Non-alloy elevated-temperature vessel plate, steel number 1.0473 As specified in EN 10028-2 Published yield 355 MPa and tensile 510–650 MPa Modern European carbon-manganese boiler and vessel plate Related strength class only

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. A later EN 10028 designation does not by itself authorize substitution. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United Kingdom (historical) BS 1501-1:1980 225 Grade 490A Same type and tensile grade with the opposite A/B suffix Not an automatic substitute; suffix B adds characteristic elevated-temperature values
Europe EN 10028-3 P355NH (1.0565) Later weldable fine-grain elevated-temperature vessel plate. Live published yield 355 MPa and tensile 490–630 MPa, against 355 N/mm² and 490–610 N/mm² for 225 Grade 490. Near name only; LT suffixes of type 225 are not automatic P355NL1 or P355NH aliases
Europe EN 10028-3 P355NL1 (1.0566) Later weldable fine-grain low-temperature vessel plate. Live published yield 355 MPa and tensile 490–630 MPa. Related strength class only
Europe EN 10028-2 P355GH (1.0473) Later non-alloy elevated-temperature vessel plate. Live published yield 355 MPa and tensile 510–650 MPa. Related strength class only
China GB/T 713 Q345R Later Chinese carbon-manganese vessel plate. Live published yield 345 MPa and tensile 510–640 MPa. Related strength class only

Why choose SHH STEEL for BS 1501-225 Grade 490B

  • We produce and export BS 1501-225 Grade 490B pressure-vessel steel plate
  • We review the enquiry for edition, designation, delivery condition, dimensions and extra tests
  • We keep the 1980 type, tensile grade and A/B suffix distinct from later EN 10028 names and from BS 1501-2 / BS 1501-3
  • We match documentation to what the purchase order requires

How to enquire for BS 1501-225 Grade 490B plate

Item What to specify
Standard and designation BS 1501-225 Grade 490B and the edition required
Or successor standard EN 10028-2 or EN 10028-3 designation and edition, if that is what the project now requires
Delivery condition Normalized, unless an alternative condition is agreed.
Dimensions Required thickness, width and length
Chemistry Ladle analysis to BS 1501-1:1980, or to another named edition
Mechanical tests Yield strength, tensile strength, elongation and, where specified, elevated-temperature or impact tests to the named edition
Other tests Ultrasonic examination or other extra tests only when written on the order
Documentation State the inspection document type required by the project

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Is BS 1501 still a current product standard?
No. BS 1501-1:1980 is the last final edition of Part 1. It was withdrawn on 15 February 1993 and replaced in the British collection by BS EN 10028-1, BS EN 10028-2, BS EN 10028-3 and BS EN 10029. Projects still using the 1980 designation should name that edition on the order.
Which edition do the tables on this page follow?
They follow BS 1501-1:1980, including tabulated values from a reprint that incorporates Amendments No. 1 to No. 3. They are not current EN 10028 tables. Specify the edition or successor standard required on the purchase order.
Does BS 1501-1 cover alloy or stainless pressure-vessel plates?
No. Part 1 covers carbon and carbon-manganese plates. Alloy plates belong to BS 1501-2:1988. Corrosion- and heat-resisting plates, sheet and strip belong to BS 1501-3:1990. Bars and sections belong to BS 1502, and forgings to BS 1503. This page is 225 Grade 490B only.
Can P355NH be used instead of 225 Grade 490B?
Only after a project review. Live P355NH is stated as 355 MPa yield and 490–630 MPa tensile, against 355 N/mm² and 490–610 N/mm² for 225 Grade 490. Suffix B elevated values remain those of BS 1501-1:1980 Appendix E. A later EN name is not an automatic substitute.
What should a quotation enquiry include?
BS 1501-225 Grade 490B, the edition required or the successor designation, the delivery condition, plate thickness by width by length, quantity, any extra tests, and the inspection document required.

Request a quotation

Contact SHH STEEL for a quotation for BS 1501-225 Grade 490B steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the edition (BS 1501-1:1980 or a named successor such as EN 10028-2 or EN 10028-3), the A or B suffix, any required impact suffix, the delivery condition and any specimen heat treatment. If your project requires ultrasonic examination, a stated impact temperature or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response