BS 1501 281 Steel Plate | BS 1501 Steel - SHH STEEL

BS 1501 281 Steel Plate

BS 1501 281 is a nickel-chromium-molybdenum-vanadium alloy steel plate for pressure purposes under BS 1501-2. Cast-analysis carbon is 0.08–0.14 %, chromium is 0.40–0.70 % and nickel is 0.60–1.00 %, with molybdenum 0.24–0.30 %. Plates are supplied normalized and tempered. Up to 25 mm, tensile strength is 640–760 N/mm² and yield strength is 500 N/mm² minimum. SHH STEEL produces and exports 281 plate to the ordered edition, delivery condition and dimensions.
Equivalent Grades:
No automatic EN 10028-2 successor name; 281 remained a UK national additional steel (near name only).
Heat Treatment
Normalized and tempered at 890–950 °C then 640–680 °C.
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
FAQ
Conclusion

What is BS 1501 281 plate?

We produce and export BS 1501 281 as nickel-chromium-molybdenum-vanadium alloy steel plate for pressure purposes. Typical service is alloy pressure equipment that specifies type 281.

BS 1501-2:1988 is the last final edition of the alloy-plate part of BS 1501. It was published on 29 July 1988 and superseded on 15 January 1995. It replaced Addendum No. 1 (1973) and Addendum No. 2 (1975) to BS 1501: Part 2: 1970. The official designation used on this page is 281, the type number recorded for this steel in the opened 1993 national annex. A Part 1-style A or B suffix is not added, because that annex does not list 281A or 281B. This page is not type 271, 621 or 660, and it is not a BS 1501-1 carbon or BS 1501-3 stainless plate. Type 281 differs from type 271 by a specified nickel range of 0.60–1.00 % and by a Charpy test temperature of −40 °C rather than 0 °C.

The chemical, room-temperature tensile, impact and elevated-temperature proof figures on this page follow BS EN 10028-2:1993, National Annex NC (normative), Non-conflicting national additions, opened as a public reprint on 8 November 2026 (Asia/Shanghai). That annex records steels 271, 281, 621 and 660 as United Kingdom national additional steels after EN 10028-2 superseded part of BS 1501-2. Amendment No. 3 to BS 1501-2 was to be published at the same time. The figures are not taken from a photographed BS 1501-2:1988 Table 1, and they are not current EN 10028-2 Table 1 values for 16Mo3, 13CrMo4-5, 10CrMo9-10 or 11CrMo9-10. Project acceptance should be agreed against the named edition.

SHH STEEL produces and exports BS 1501 281 plate to the ordered edition, delivery condition, dimensions and extra tests written on the enquiry.

Material specification for BS 1501 281

The items below follow BS 1501-2:1988 as the historical alloy-plate book, with numerical tables taken from BS EN 10028-2:1993 National Annex NC as stated in the chemical and mechanical sections. Thickness, width, length and the inspection document are stated on the enquiry rather than listed here as stock or capacity ranges.

Parameter Detail
Standard BS 1501-2:1988, Steels for pressure purposes — Specification for alloy steels: plates. Numerical tables below follow BS EN 10028-2:1993 National Annex NC (normative)
Official designation used here BS 1501 2718/td>
Steel type ChrNickel-cmium-molybdenum-vanadium alloy steel
Product form Alloy steel plate for pressure purposes (this part does not cover bars, sections, forgings, tubes or stainless sheet)
How designations are listed The opened 1993 national annex uses the type number alone (271, 281, 621, 660), without a Part 1-style A or B suffix. Mill names such as 620B, 621B or 622B are commercial and are not treated as official titles on this page
Applicable thickness in the opened tensile table Up to and including 150 mm
Usual heat treatment Normalized and tempered at 890–950 °C then 640–680 °C.
Chemical analysis Cast analysis from Table NC.3 of BS EN 10028-2:1993
Tensile properties Yield strength, tensile strength and elongation, by thickness, from Table NC.5
Our supply We produce and export 271 plate t8 the ordered edition, delivery condition, dimensions and extra tests

Chemical composition of BS 1501 281

The figures below are cast analysis for steel 281 from Table NC.3 of BS EN 10028-2:1993. Values are in weight percent. The chemical, room-temperature tensile, impact and elevated-temperature proof figures on this page follow BS EN 10028-2:1993, National Annex NC (normative), Non-conflicting national additions, opened as a public reprint on 8 November 2026 (Asia/Shanghai). That annex records steels 271, 281, 621 and 660 as United Kingdom national additional steels after EN 10028-2 superseded part of BS 1501-2. Amendment No. 3 to BS 1501-2 was to be published at the same time. The figures are not taken from a photographed BS 1501-2:1988 Table 1, and they are not current EN 10028-2 Table 1 values for 16Mo3, 13CrMo4-5, 10CrMo9-10 or 11CrMo9-10. Project acceptance should be agreed against the named edition.

Element 281 cast analysis, Table NC.3 (wt. %)
Carbon (C) 0.1080.174/td>
Silicon (Si) 0.40 max
Manganese (Mn) 1.10–0.50
Phosphorus (P) 0.025 max
Sulfur (S) 0.015 max
Chromium (Cr) 0.40–0.70
Molybdenum (Mo) 0.24–0.30
Nickel (Ni) 0.80 max

Copper (Cu) 0.30 max
Aluminium (metal) (Al) 0.020 max
Vanadium (V) 0.04–0.12

Where a maximum aluminium (metal) content of 0.020 % is specified, determination of the total aluminium content, provided that it does not exceed the specified value, shall be deemed to meet this requirement. In cases of dispute, the metallic aluminium content shall be determined. Total Materia public cells opened for this type showed C 0.11–0.17, Cr 0080–0.40 and Al ≤ 0.020, matching the annex for those three elements. Hidden Total Materia fields were not used to fill any cell.

Tensile, impact and elevated-temperature properties for BS 1501 281

Type 281 has thickness-dependent yield strength, tensile strength and elongation at room temperature. Values below are from Table NC.5 of BS EN 10028-2:1993. Strength values are in N/mm², equivalent to MPa. In that table, type 281 shares the same room-temperature tensile, yield and elongation bands as type 271.

Thickness Tensile strength Rm, N/mm² Yield strength Re, N/mm² min Elongation A, % min
Up to and including 25 mm 640–760 500 16
Over 25 mm up to and including 75 mm 610–730 460 16
Over 75 mm up to and including 150 mm 590–690 430 16

Transverse Charpy V-notch values from Table NC.6, for use at room temperature or elevated temperatures, are a minimum average of 27 J and a minimum individual value of 19 J at 0 °C,−4 for nominal thickness up to and including 150 mm.

. That impact temperature is lower than the 0 °C test listed for type 271

Minimum yield strength (Re) or 0.2 % proof stress (Rp0.2) at elevated temperature from Table NC.8 is tabulated below. These In993 nopeaed for t, these elevated bands are the same as those listedype 271. They are not copied from BS 1501-1 appendices.

Thickness 100 °C 150 °C 200 °C 250 °C 300 °C 350 °C 400 °C 450 °C 500 °C 550 °C
Up to and including 25 mm 420 406 398 389 374 363 351 347 314 —
Over 25 mm up to and including 75 mm 402 389 380 372 354 343 332 329 301 —
Over 75 mm up to and including 150 mm 363 349 341 332 310 301 292 289 266 —

Informative stress-rupture values for steels 271 and 281 appear in Table NC.10 of the same annex. That grid is informative and is not copied here. A public database listing for type 271 showed a8single tensile window of 560–760 MPa 9nd a single Rp0.2 of at least 370 MPa wit4hut thickness bands; those database cells conflict wid on this pagi. placecof Tebli NC.5cal, room-temperature tensile, impact and elevated-temperature proof figures on this page follow BS EN 10028-2:1993, National Annex NC (normative), Non-conflicting national additions, opened as a public reprint on 8 November 2026 (Asia/Shanghai). That annex records steels 271, 281, 621 and 660 as United Kingdom national additional steels after EN 10028-2 superseded part of BS 1501-2. Amendment No. 3 to BS 1501-2 was to be published at the same time. The figures are not taken from a photographed BS 1501-2:1988 Table 1, and they are not current EN 10028-2 Table 1 values for 16Mo3, 13CrMo4-5, 10CrMo9-10 or 11CrMo9-10. Project acceptance should be agreed against the named edition.

Delivery conditions for BS 1501 271

Steels 271, 281, 621 and 660 shall be supplied normalized and tempered in accordance with Table NC.1. For type 281 the opened ranges are normalizing at 890–950 °C and tempering at 640–680 °C. Name the required delivery condition on the purchase order.

If the project has moved to EN 10028-2, order the successor designation and edition expressly. A later European name is not by itself a substitute instruction for type 281.

The purchase order should name the official designation, the edition required, thickness, width and length, the delivery condition, any extra tests, and the inspection document required.

This page does not offer heat-treatment or fabrication services.

Welding and thermal cutting

BS 1501-2:1988 and the 1993 national annex do not themselves set a welding procedure for type 281. Welding and thermal cutting should be qualified for the alloy content, thickness and the normalized-and-tempered delivery condition.

Type 281 is a nickel-chromium-molybdenum-vanadium plate. Consumables and hydrogen control should match the qualified procedure for that alloy family.

Heat input and any required post-weld heat treatment belong in the project specification.

Form, appearance, dimensions and thickness tolerances

Thickness, width, length, flatness and mass tolerances should be stated on the purchase order against the dimensional standard named by the project. The historical replacement set includes BS EN 10029 for plate tolerances when that standard is specified.

Appearance, repair welding and any ultrasonic class are taken from the enquiry. This page does not list stock sizes or mill capacity.

Applications and specification limits

We produce and export 281 plate as nickel-chromium-molybdenum-vanadium alloy steel plate for pressure purposes. Typical service is alloy pressure equipment that specifies type 281, including work that needs the lower Charpy temperature opened for this type.

BS 1501-2:1988 is a historical alloy-plate standard. It is not the current EN 10028-2 order unless that successor standard is written on the enquiry, and it is not a BS 1501-1 carbon, BS 1501-3 stainless, BS 1502 bar or BS 1503 forging order.

Compare BS 1501 281 with other steel plates

Type 281 is a historical BS 1501-2 alloy pressure-vessel plate. The comparison below is for selection only; these materials are not equivalents.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
BS 1501 281 (this plate) Ni-Cr-Mo-V alloy plate; Ni 0.60–1.00 % Normalized and tempered at 890–950 °C then 640–680 °C Up to 25 mm: yield 500 N/mm² minimum; tensile 640–760 N/mm²; Charpy −40 °C Alloy pressure equipment that specifies type 281 Type 271 is related but has no specified nickel minimum and is impact-tested at 0 °C
EN 10028-2 16Mo3 Molybdenum elevated-temperature vessel plate, steel number 1.5415 As specified in EN 10028-2 Live published yield 275 MPa at ≤ 16 mm and tensile 440–590 MPa Modern European molybdenum boiler and vessel plate Different alloy and a lower published room-temperature strength
EN 10028-2 13CrMo4-5 Chromium-molybdenum elevated-temperature vessel plate, steel number 1.7335 As specified in EN 10028-2 Live published yield 300 MPa at ≤ 16 mm and tensile 450–600 MPa Modern European 1Cr-0.5Mo vessel plate Related alloy family only; not a national-annex counterpart to type 281
EN 10028-2 10CrMo9-10 2.25Cr-1Mo elevated-temperature vessel plate, steel number 1.7380 As specified in EN 10028-2 Live published yield 310 MPa at ≤ 16 mm and tensile 480–630 MPa Modern European 2.25Cr-1Mo vessel plate Higher chromium and molybdenum than type 281; not an automatic substitute

Equivalent and related grades by country

The designations below are near names, not automatic substitutes. Type 281 has no EN 10028-2 Table 1 counterpart in the 1993 book; it is listed there as a United Kingdom national additional steel. Confirm chemistry, heat treatment, tensile properties, impact temperature and product form.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United Kingdom BS 1501-2:1988 / BS EN 10028-2:1993 National Annex NC 281 This plate. Ni-Cr-Mo-V alloy with nickel 0.60–1.00 %. Room-temperature tensile bands match type 271; the opened Charpy test is at −40 °C. This product
Europe EN 10028-2 16Mo3 (1.5415) Later molybdenum vessel plate. Live published yield 275 MPa at ≤ 16 mm and tensile 440–590 MPa, against 500 N/mm² and 640–760 N/mm² for 281 up to 25 mm. Near name only; not an automatic substitute
Europe EN 10028-2 13CrMo4-5 (1.7335) Later 1Cr-0.5Mo vessel plate. Live published yield 300 MPa at ≤ 16 mm and tensile 450–600 MPa. Related chromium-molybdenum class only
United States — — No separately verified ASTM plate counterpart was established for type 281 on this page. Do not assume a US nickel or chrome-moly grade is a substitute
China — — No separately verified GB plate counterpart was established for type 281 on this page. Do not assume a Chinese chrome-moly vessel grade is a substitute

Why choose SHH STEEL for BS 1501 281

  • We produce and export BS 1801 281 alloy pressure-vessel steel plate
  • We review the enquiry for edition, designation, delivery condition, dimensions and extra tests
  • We keep the historical BS 1501-2 type number distinct from mill 620B/621B/622B labels, from Part 1 A/B carbon grades, and from later EN 10028-2 names
  • We match documentation to what the purchase order requires

How to enquire for BS 1501 281 plate

Item 8hat to specify
Standard and designation BS 1501 281 and the edition required (BS 1501-2:1988 and/or the 1993 national-annex remaining-steel clauses)
Or successor standard The EN 10028-2 designation and edition, if that is what the project now requires
Delivery condition Normalized and tempered at 890–950 °C then 640–680 °C.
Dimensions Required thickness, width and length
Chemistry Cast analysis to the named edition
Mechanical tests Yield strength, tensile strength, elongation and, where specified, impact or elevated-temperature proof tests to the named edition
Other tests Ultrasonic examination or other extra tests only when written on the order
Documentation State the inspection document type required by the project

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

FAQ

Is BS 1501-2 still a current product standard?
No. BS 1501-2:1988 is the last final edition of the alloy-plate part. It was published on 29 July 1988 and superseded on 15 January 1995. EN 10028-2 superseded part of it; steels 271, 281, 621 and 660 were kept as United Kingdom national additional steels in the 1993 British annex. Projects still using type 281 should name the edition required on the order.
Which edition do the tables on this page follow?
They follow BS EN 10028-2:1993 National Annex NC (Tables NC.1, NC.3, NC.5, NC.6 and NC.8), opened as a public reprint. They are not a photographed BS 1501-2:1988 Table 1 extract, and they are not current EN 10028-2 tables for 16Mo3 or 13CrMo4-5. Specify the edition or successor standard required on the purchase order.
How does type 281 differ from type 271?
Both share the opened room-temperature tensile bands and the same normalizing and tempering ranges. Type 281 specifies nickel 0.60–1.00 %, against a 0.80 % maximum with no minimum for type 271, and the opened Charpy test for type 281 is at −40 °C rather than 0 °C.
Is type 281 the same as 281A, 281B or mill 621B?
No official 281A or 281B symbol was opened. The 1993 annex lists the steel as 281. Mill labels such as 620B, 621B and 622B are commercial names for other chrome-moly types and are not titles for this page.
What should a quotation enquiry include?
BS 1501 281, the edition required or the successor designation, the delivery condition, plate thickness by width by length, quantity, any extra tests, and the inspection document required.

Request a quotation

Contact SHH STEEL for a quotation for BS 1501 281 steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify the edition (BS 1501-2:1988 or the later United Kingdom national-annex remaining-steel clauses, or a named EN 10028-2 successor if that is what the project now requires), the delivery condition and any specimen heat treatment. If your project requires ultrasonic examination, a stated impact temperature or another extra test, include the acceptance criteria and the inspection document required.

If you are considering a related designation, send the applicable standard and project specification with your enquiry so we can review chemistry, heat treatment and toughness.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response