ASTM B265 Grade 31 Titanium Plate | Ti-0.3Co-0.05Pd (UNS R53532)
What is ASTM B265 Grade 31 titanium plate?
ASTM B265 Grade 31 titanium plate is made to ASTM B265, the ASTM specification for titanium and titanium alloy strip, sheet and plate. It carries the UNS number R53532. Grade 31 is Ti-0.3Co-0.05Pd at a higher oxygen level than Grade 30, giving Grade 3 strength with the same corrosion benefit.
This grade belongs to the corrosion-resistant alloyed group: its base is commercially pure titanium, and small additions such as palladium, ruthenium, nickel, molybdenum, cobalt, chromium or tantalum change how the oxide film behaves in reducing acids and tight crevices. Strength still depends mainly on oxygen and iron, so mechanical properties track the matching CP strength level, and the material is used in the annealed condition.
Its typical density of about 4.51 g/cm³ is a little over half that of carbon steel, which is one reason titanium plate is chosen where weight matters.
ASTM B265 groups its grades into unalloyed titanium, corrosion-resistant grades with small additions of palladium, ruthenium, nickel or molybdenum, and structural alloys such as Ti-3Al-2.5V and Ti-6Al-4V. Each grade has its own UNS number, and the H grades add a higher guaranteed tensile strength for pressure vessel use.
SHH STEEL handles Grade 31 plate enquiries within its range of titanium alloy plates and sheets, checking the ordered ASTM B265 edition, product form and certificate type before confirming supply. Related designations covered on this site include ASME SB-265 Grade 31, JIS H4600 Class 20 TP450PCo.
Material specification for ASTM B265 Grade 31
ASTM B265 classifies flat titanium products by thickness and width. The same chemistry and tensile requirements apply to strip, sheet and plate, but dimensional tolerances and bend testing differ by product form.
| Ordering item | ASTM B265 basis |
|---|---|
| Standard | ASTM B265, Titanium and Titanium Alloy Strip, Sheet, and Plate; state the edition on the order |
| Grade / UNS | Grade 31, Ti-0.3Co-0.05Pd, UNS R53532 |
| Plate | Over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide |
| Sheet | 0.187 in (4.75 mm) and under, 24 in (610 mm) wide or more; state cold or hot rolled |
| Strip | 0.187 in (4.75 mm) and under, less than 24 in (610 mm) wide |
| Condition | Annealed |
| Certificate | Manufacturer’s report with chemical analysis, tensile results and other required tests |
Order information listed by the specification includes grade, product limitations, special mechanical properties, marking, finish, packaging, any additional reports and the disposition of rejected material. For ASME Code construction, order to ASME SB-265 Grade 31 and state any dual certification on the purchase order.
Chemical composition of ASTM B265 Grade 31 (UNS R53532)
Single values are maximums; ranges are shown where an element is added. Titanium is determined by difference. Product analysis tolerances cover variation between laboratories and do not broaden the heat analysis limits.
| Element | Heat analysis, % | Permissible variation in product analysis, % |
|---|---|---|
| Nitrogen (N) | 0.05 | +0.02 |
| Carbon (C) | 0.08 | +0.02 |
| Hydrogen (H) | 0.015 | +0.002 |
| Iron (Fe) | 0.30 | +0.15 |
| Oxygen (O) | 0.35 | +0.04 |
| Cobalt (Co) | 0.20–0.80 | ±0.05 |
| Palladium (Pd) | 0.04–0.08 | ±0.005 |
| Other elements, each | 0.1 | +0.02 |
| Other elements, total | 0.4 | — |
| Titanium (Ti) | Balance | — |
Ingot top and bottom are analysed for the listed elements. Hydrogen is tested and reported on at least one final product sample, and a lower hydrogen limit may be negotiated. Other elements need not be reported unless they exceed 0.10% each or 0.40% total, and they may not be added intentionally.
Mechanical properties of ASTM B265 Grade 31
The values below are the requirements for Grade 31 plate in the annealed condition.
| Property | Requirement |
|---|---|
| Tensile strength, min | 65 ksi (450 MPa) |
| Yield strength, 0.2% offset | 55–80 ksi (380–550 MPa) |
| Elongation in 2 in or 50 mm, min | 18% |
| Bend test, under 0.070 in (1.8 mm) | Mandrel radius 2T, bent 105° without outside fracture |
| Bend test, 0.070–0.187 in (1.8–4.75 mm) | Mandrel radius 2.5T |
| Bend test, over 0.187 in (4.75 mm) | Not applicable to material over 4.75 mm |
Tensile tests are made at room temperature. The yield range has an upper limit as well as a lower one. That cap protects formability, so a plate with very high yield can fail the grade even if it is strong. Bend tests apply to sheet and strip up to 0.187 in (4.75 mm); plate over that thickness is not bend tested under the specification.
Elevated-temperature design values are not part of the plate specification. They come from the design code, such as ASME Section II, Part D where the grade is listed.
Delivery condition, finish and marking
ASTM B265 covers material in the annealed condition. Plate must be free of injurious external and internal imperfections. Annealed product may be furnished descaled, sandblasted, ground, or sandblasted and ground; state the finish on the order.
- Condition: Annealed
- Surface: descaled, sandblasted or ground, as ordered; minor spot grinding is permitted within the thickness tolerance
- Marking: specification, grade, heat number, manufacturer’s identification and nominal thickness, in rows that can be removed with hot alkaline cleaning
- Packaging: boxed, crated, boarded or as the manufacturer’s standard practice unless the order states otherwise
The grade is supplied annealed and is not strengthened by heat treatment. If the plate will be formed or welded in your shop, say so at enquiry so the finish and protective packing suit the next process.
Welding and fabrication of Grade 31 titanium plate
Grade 31 is welded in the same way as CP titanium, by gas tungsten arc, plasma arc or other inert-gas processes with full shielding of the weld pool, the hot heat-affected zone and the root.
- Use trailing shields and back purging until the metal cools below about 400 °C
- Select filler metal that keeps the alloying addition in the weld, normally matching filler, so the weld does not become the least corrosion-resistant zone
- Keep joints, wire and gloves clean; avoid iron contamination from carbon steel tools
- Check weld colour and reject heavily discoloured welds
Forming behaviour is close to the CP grade of the same oxygen level. Allow for springback, and keep forming tools clean so iron is not smeared into the surface.
For machining, use sharp tools, low cutting speeds, steady feeds and plenty of coolant, as for CP titanium. Keep chips separate by grade so the alloying addition can be traced in scrap, and do not let fine chips accumulate, because titanium fines can ignite.
These are general practices, not a qualified procedure. The fabricator must qualify the welding procedure, filler metal and inspection to the applicable code.
Dimensional tolerances and flatness
Dimensional tolerances are set in the specification’s tables for thickness, width, length, weight and flatness. Plate flatness has its own table for annealed plate. For sheet, cold-rolled tolerances apply unless hot-rolled sheet is ordered.
State the nominal thickness, width, length, quantity and any cutting drawing at enquiry. If a project needs tighter flatness, a specific edge condition or cut-to-size pieces, write it on the order rather than relying on the default tables. No stock sizes are implied by this page.
Titanium plate can be cut by waterjet, abrasive saw, plasma or machining. Thermal cutting leaves an oxygen-enriched edge that should be removed by machining or grinding before welding or forming, so agree the cut-edge condition and any machining allowance on the order.
Applications and service limits of Grade 31 titanium plate
Typical uses of Grade 31 plate include:
- Equipment handling hot chloride brines where crevice corrosion is a risk
- Reactors and vessels in mildly reducing acids such as dilute hydrochloric or sulfuric acid
- Flue gas desulfurisation and chemical process heat exchangers
- Gasket faces, flange areas and crevice-prone parts of titanium equipment
Formability is lower than Grade 30. The alloying addition improves resistance in mildly reducing acids and hot chloride crevices, but it does not make titanium suitable for hydrofluoric acid, fluoride-bearing media, dry chlorine, strongly reducing hot concentrated acids or red fuming nitric acid. Corrosion performance depends on acid concentration, temperature, aeration and impurities, so the design engineer should confirm the grade with corrosion data or tests for the actual medium.
When selecting Grade 31, compare it with Grade 12, Grade 13, Grade 14. The choice usually turns on the balance of strength, formability, corrosion behaviour in the actual medium and cost, and on which standard the drawing or design code names.
Compare Grade 31 with other ASTM B265 grades
The grades below are the closest neighbours of Grade 31 in ASTM B265. Values are tensile strength, 0.2% yield or proof strength and minimum elongation, as set by the standard.
| Grade | Tensile strength | Yield / proof strength | Elongation, min | Typical role |
|---|---|---|---|---|
| Grade 12 (R53400) | 70 ksi (483 MPa) | 50 ksi (345 MPa) min | 18% | Ni-Mo alloy for hot brines |
| Grade 13 (R53413) | 40 ksi (275 MPa) | 25 ksi (170 MPa) min | 24% | Ni-Ru, lowest strength |
| Grade 14 (R53414) | 60 ksi (410 MPa) | 40 ksi (275 MPa) min | 20% | Ni-Ru, medium strength |
| Grade 15 (R53415) | 70 ksi (483 MPa) | 55 ksi (380 MPa) min | 18% | Ni-Ru, highest strength |
| Grade 30 (R53530) | 50 ksi (345 MPa) | 40–65 ksi (275–450 MPa) | 20% | Co-Pd, Grade 2 strength |
| Grade 31 (R53532) | 65 ksi (450 MPa) | 55–80 ksi (380–550 MPa) | 18% | Co-Pd, Grade 3 strength |
| Grade 33 (R53442) | 50 ksi (345 MPa) | 40–65 ksi (275–450 MPa) | 20% | Ni-Pd-Ru-Cr, Grade 2 strength |
| Grade 34 (R53445) | 65 ksi (450 MPa) | 55–80 ksi (380–550 MPa) | 18% | Ni-Pd-Ru-Cr, Grade 3 strength |
The grades in this group differ in the alloying addition and in oxygen level. The addition sets the corrosion behaviour and cost; the oxygen level sets strength and formability. A change of grade should be approved by the engineer responsible for corrosion design.
ASTM B265 Grade 31 equivalent grades
The designations below are commonly compared with ASTM B265 Grade 31. They are close in composition and role, but limits, tests and product forms are set by each standard, so they are not automatically interchangeable.
| Standard / system | Designation | Relationship to ASTM B265 Grade 31 |
|---|---|---|
| ASME SB-265 | Grade 31 | ASME Code adoption of B265; ordered for pressure equipment |
| JIS H4600 | Class 20 (TP450PCo) | Close equivalent; JIS strength range and tests differ |
| UNS | R53532 | Same unified number as ASTM Grade 31 |
Where a drawing names one designation and the supplier offers another, agree in writing which standard governs chemistry, tensile values, testing and marking. Dual or multiple certification is possible only when the material meets every cited standard in full, and the certificate must show the results against each one.
Why choose SHH STEEL for Grade 31 titanium plate
SHH STEEL supports specification-led purchasing of titanium plate and sheet.
- We quote to the ASTM B265 edition, grade and product form you name, and keep B265 and SB-265 requirements distinct
- Certificates are checked against the Grade 31 chemistry and tensile limits, including the yield upper limit
- Sizes, quantities, testing and delivery are confirmed in the quotation, not assumed
- Finish, marking and packing are agreed before production
Questions on equivalents, dual certification or edition changes are answered before an order is placed.
How to enquire for ASTM B265 Grade 31 plate
Send the material schedule with the details below. We review the enquiry and raise any open points before confirming the supply route.
| Enquiry item | Information required |
|---|---|
| Material | ASTM B265 Grade 31 (UNS R53532), edition; add ASME SB-265 if Code use |
| Product form | Plate, sheet or strip; for sheet, cold or hot rolled |
| Dimensions | Thickness, width, length, quantity and any cutting drawing |
| Finish | Descaled, sandblasted, ground or other agreed surface |
| Testing | Any special mechanical properties, extra analysis or reports |
| Documents | Certificate type and any third-party inspection |
| Destination | Delivery place and packing requirements |
FAQ
-
Is ASTM B265 Grade 31 the same as ASME SB-265 Grade 31?
- SB-265 is the ASME Code adoption of B265, so Grade 31 requirements normally match. They are separate documents, and ASME may adopt a different edition. For Code work, order SB-265 Grade 31 or dual certification.
-
What is the tensile strength of ASTM B265 Grade 31 titanium plate?
- The requirement is 65 ksi (450 MPa) minimum. The 0.2% proof or yield strength is 55–80 ksi (380–550 MPa). Minimum elongation is 18%. Values apply to the condition and thickness range stated in the standard.
-
What is Grade 31 mainly used for?
- Typical uses include equipment handling hot chloride brines where crevice corrosion is a risk, reactors and vessels in mildly reducing acids such as dilute hydrochloric or sulfuric acid and flue gas desulfurisation and chemical process heat exchangers. Formability is lower than Grade 30.
-
When is a titanium product classed as plate under B265?
- Plate is over 0.187 in (4.75 mm) thick and over 10 in (254 mm) wide. Thinner product is sheet if 24 in (610 mm) wide or more, otherwise strip.
-
What should I send for a quotation?
- Send ASTM B265 Grade 31, the edition, product form, thickness, width, length and quantity, the finish, any special testing, the certificate type and the destination. Add ASME SB-265 if the plate is for Code construction.
Request a quotation for ASTM B265 Grade 31 titanium plate
ASTM B265 Grade 31 is Ti-0.3Co-0.05Pd titanium, UNS R53532, specified for 65 ksi (450 MPa) minimum tensile strength, 55–80 ksi (380–550 MPa) yield or proof strength and 18% minimum elongation in the annealed condition. Typical uses include equipment handling hot chloride brines where crevice corrosion is a risk and reactors and vessels in mildly reducing acids such as dilute hydrochloric or sulfuric acid.
Send the product form, sizes, quantity, finish, certificate type and destination to SHH STEEL. Compare other grades on the ASTM B265 page or browse all titanium alloy plates and sheets. Availability, testing and delivery are confirmed against each enquiry.
Contact: admin@steelspecs.com