ASTM A553 Type III 7% Nickel Steel Plate | ASTM A553 Nickel Steel - SHH STEEL

ASTM A553 Type III 7% Nickel Steel Plate

ASTM A553 Type III is quenched and tempered 7% nickel steel plate. The current ASTM publication, A553/A553M-22, lists Type I (9% nickel), Type II (8% nickel) and Type III (7% nickel). Type III is impact tested at −320 °F [−195 °C] unless another temperature is agreed. Thickness is limited only by the ability of the plate to meet the specified mechanical properties. SHH STEEL produces and exports ASTM A553 Type III plate to the edition and heat treatment named on the order.
Equivalent Grades:
ASME SA553 Type III; 06Ni7DR (7% nickel). Edition, condition and tests differ; not automatic substitutes.
Heat Treatment
Water quenched and tempered (A553/A553M-17 reference; ASME 2023 adoption).
Share:
General Description
Material Specification
Chemical Composition
Mechanical Properties
Delivery Conditions
Weldability
Tolerances
Applications and service limits
Compare
Equivalent Material Grade
Why choose Us
Our Service
Conclusion

What is ASTM A553 Type III steel plate?

ASTM A553 Type III is water-quenched and tempered 7% nickel alloy steel plate to ASTM A553/A553M. The current ASTM publication is A553/A553M-22. The official title covers quenched and tempered 7%, 8% and 9% nickel plates. The official split is Type I, Type II and Type III — not Grade and not Class.

Type III is the 7% nickel type. An ASTM A553 order that does not name the Type is incomplete. Writing only Type I and Type II would not cover the current specification. This page does not claim that current ASTM A553/A553M-22 is the same document as ASME SA-553 (identical with A553/A553M-17 in BPVC.II.A-2023).

SHH STEEL produces and exports ASTM A553 Type III 7% nickel steel plate to the ordered edition, heat treatment, dimensions and extra tests written on the enquiry. This plate belongs to our Boiler & Pressure Vessel Steel Plates range under ASTM A553.

Material specification for ASTM A553 Type III

Type identification from the ASTM A553/A553M-22 store scope, with table values cited as noted below.

Parameter Detail
Standard ASTM A553/A553M-22, Standard Specification for Pressure Vessel Plates, Alloy Steel, Quenched and Tempered 7%, 8%, and 9% Nickel
Official split Type III (nominal 7% nickel). The specification uses Type, not Grade or Class
Complete official types in this specification Type I = 9% nickel; Type II = 8% nickel; Type III = 7% nickel. This page specifies Type III
Product form Pressure-vessel steel plate, water quenched and tempered
General requirements ASTM A20/A20M; A553/A553M prevails in a conflict
Steelmaking Killed steel; fine austenitic grain size
Chemical analysis Table 1 for Type III from ASTM A553/A553M-17 as published in ASME BPVC.II.A-2023 SA-553/SA-553M, including molybdenum 0.10–0.30 and niobium 0.03 max; not presented as the A553/A553M-22 text
Delivery condition Water quenched and tempered; QT marking, or QTT when the optional intermediate treatment is used
Thickness ASTM A553/A553M-22 scope: limited only by the capacity of the material to meet the specified mechanical property requirements
Impact testing Mandatory Charpy V-notch at −320 °F [−195 °C] unless another temperature is agreed; lateral expansion not less than 0.015 in. [0.381 mm]
Units Inch-pound and SI values are separate standards; do not combine them
Our supply We produce and export ASTM A553 Type III plate to the ordered edition, heat treatment, dimensions and extra tests

Official types in ASTM A553/A553M-22:

Type Nominal nickel, % Default impact test temperature
I 9 −320 °F [−195 °C]
II 8 −275 °F [−170 °C]
III 7 −320 °F [−195 °C]

Chemical composition of ASTM A553 Type III

The current ASTM publication is A553/A553M-22. Its published scope lists three types — Type I (nominal 9% nickel), Type II (nominal 8% nickel) and Type III (nominal 7% nickel) — and requires impact testing at −320 °F [−195 °C] for Type I or Type III and at −275 °F [−170 °C] for Type II, unless another temperature is agreed. Maximum thickness is limited only by the capacity of the material to meet the specified mechanical property requirements.

The chemical composition, tensile values and heat-treatment temperatures below are those of ASTM A553/A553M-17, as published in ASME BPVC Section II, Part A, 2023 under SA-553/SA-553M (identical with A553/A553M-17). They are not presented as the A553/A553M-22 text.

Name the edition required on the purchase order: ASTM A553/A553M-22, ASME SA-553/SA-553M in the stated Section II year, or both when dual documents are required. We produce and export to the documents named on the order.

Element Type III heat analysis (wt. %) Type III product analysis (wt. %)
Carbon (C), max 0.13 0.13
Manganese (Mn), max 0.90 0.98
Phosphorus (P), max 0.010 0.010
Sulfur (S), max 0.010 0.010
Silicon (Si) 0.05–0.30 0.05–0.30
Nickel (Ni) 6.50–7.50 6.50–7.50
Molybdenum (Mo) 0.10–0.30 0.10–0.30
Columbium / niobium (Nb), max 0.03 0.03

Carbon, phosphorus, sulfur, molybdenum and niobium limits carry footnote A in SA-553 Table 1 (identical with A553/A553M-17): they apply to both heat and product analyses. Type III silicon 0.05–0.30 and nickel 6.50–7.50 also carry footnote A on the heat-analysis cell; the product-analysis cells in those printed rows are blank because the same range applies to both analyses, not because a second range is missing. Columbium and niobium are interchangeable names for the same element. These figures are the A553/A553M-17 / SA-553 2023 table as published in ASME BPVC.II.A-2023 SA-553/SA-553M, not an SHH STEEL proprietary chemistry. They are not presented as the A553/A553M-22 text.

Tensile and impact requirements for ASTM A553 Type III

The current ASTM publication is A553/A553M-22. Its published scope lists three types — Type I (nominal 9% nickel), Type II (nominal 8% nickel) and Type III (nominal 7% nickel) — and requires impact testing at −320 °F [−195 °C] for Type I or Type III and at −275 °F [−170 °C] for Type II, unless another temperature is agreed. Maximum thickness is limited only by the capacity of the material to meet the specified mechanical property requirements.

The chemical composition, tensile values and heat-treatment temperatures below are those of ASTM A553/A553M-17, as published in ASME BPVC Section II, Part A, 2023 under SA-553/SA-553M (identical with A553/A553M-17). They are not presented as the A553/A553M-22 text.

Name the edition required on the purchase order: ASTM A553/A553M-22, ASME SA-553/SA-553M in the stated Section II year, or both when dual documents are required. We produce and export to the documents named on the order.

Table 2 in the A553/A553M-17 / SA-553 2023 text lists one tensile package for the specification; it is not split by Type. Nickel content, some chemistry limits, tempering range and default impact temperature still differ by Type.

Property Requirement (A553/A553M-17 as in SA-553, 2023)
Tensile strength 100–120 ksi [690–825 MPa]
Yield strength (0.2% offset), min 85 ksi [585 MPa]
Elongation in 2 in. [50 mm], min 20.0% (see A20/A20M for elongation adjustment)
Impact test method Charpy V-notch to A20/A20M
Specimen orientation Longitudinal axis of the specimen transverse to the final rolling direction
Default test temperature for Type III −320 °F [−195 °C], unless otherwise agreed
Mandatory acceptance Each specimen: lateral expansion opposite the notch not less than 0.015 in. [0.381 mm]

Optional S55 and S56 energy-absorption requirements apply only when ordered. They are not the default mandatory impact criterion.

Heat treatment for ASTM A553 Type III

Plates are supplied in the water-quenched and tempered condition. Shell plates and other parts heated for forming shall be heat treated after forming to the same procedure.

  • Hardening: heat to a suitable temperature in the range 1475–1700 °F [800–925 °C], hold long enough to obtain a uniform temperature through the thickness, and quench in water (the detailed hardening clause also says quench in a liquid medium).
  • Tempering 1000–1125 °F [540–615 °C] for Type III: hold at least 30 min/in. [1.2 min/mm] of thickness and not less than 15 min, then cool in air or quench at a rate not less than 300 °F/h [165 °C/h].

Before tempering, plates may receive an optional intermediate heat treatment (1205–1330 °F [650–720 °C] for Type III), held at least 15 min, then cooled as specified by thickness in the standard. When that optional treatment is used, plates are marked QTT instead of QT. The intermediate treatment may be performed at the manufacturer option or specified by the purchaser. This page does not offer heat-treatment or fabrication services.

The heat-treatment temperatures above are those of ASTM A553/A553M-17 as published in ASME BPVC.II.A-2023 SA-553/SA-553M. Type III tempering is 1000–1125 °F [540–615 °C], which is not the Type I / Type II range. These temperatures are not presented as the A553/A553M-22 text.

Water quenched and tempered: heat 1475–1700 °F [800–925 °C] and water quench; temper 1000–1125 °F [540–615 °C] for Type III, hold at least 30 min/in. [1.2 min/mm] and not less than 15 min, then air cool or quench at not less than 300 °F/h [165 °C/h]. Optional intermediate treatment 1205–1330 °F [650–720 °C] is marked QTT. Temperatures are those of ASTM A553/A553M-17 as published in ASME BPVC.II.A-2023 SA-553/SA-553M; they are not presented as the A553/A553M-22 text.

Welding and handling notes

ASTM A553 covers plates intended for the fabrication of welded pressure vessels. Welding procedures and any post-weld heat treatment belong to the project specification and the fabricator. This page does not offer fabrication or procedure qualification.

The specification warns that the material is susceptible to magnetization and that magnets should be avoided in handling after heat treatment if residual magnetism would be detrimental.

General requirements, marking and dimensions

Material supplied to ASTM A553/A553M shall conform to ASTM A20/A20M except where A553/A553M prevails. In the A553-17 / SA-553 text, each plate is marked QT, or QTT when the optional intermediate heat treatment is used. Dimensional tolerances are those of the ordered A20/A20M edition and the mill documents, not a stock list.

Applications and specification limits

We produce and export this plate for projects that specify ASTM A553/A553M Type III. The specification is written for welded pressure vessels in the water-quenched and tempered condition. This page does not treat Type I, Type II and Type III as interchangeable.

Compare ASTM A553 Type III with related nickel steel plates

Type III is an official type in the current ASTM A553/A553M-22 scope and in SA-553 (identical with A553/A553M-17). It is not an extra commercial grade invented beside Type I and Type II. Type I and Type II remain separate types with different nickel windows and, for Type II, a different default impact temperature. Type III also uses a different tempering range and adds molybdenum and niobium limits.

Material Alloy / type Delivery condition Mechanical requirements Typical service Substitution limit
ASTM A553 Type III (this plate) Official Type III, nominal 7% nickel; not a Grade or Class Water quenched and tempered; temper 1000–1125 °F [540–615 °C]; optional intermediate treatment marked QTT Tensile 100–120 ksi [690–825 MPa]; yield 85 ksi [585 MPa] min; impact −320 °F [−195 °C]; lateral expansion not less than 0.015 in. [0.381 mm] Welded pressure vessels specified to A553 Type III Do not substitute Type I, Type II, A353 or 06Ni7DR without a project review
ASTM A553 Type I 9% nickel steel plate Official Type I, nominal 9% nickel Water quenched and tempered; temper 1050–1175 °F [565–635 °C] Same tensile table in the A553-17 / SA-553 text; default impact −320 °F [−195 °C]; no molybdenum or niobium requirement in Table 1 for Type I Orders written to Type I Different nickel window, phosphorus/sulfur maxima and tempering range. Not Type III
ASTM A553 Type II 8% nickel steel plate Official Type II, nominal 8% nickel Water quenched and tempered; same tempering range as Type I Same tensile table; default impact −275 °F [−170 °C] Orders written to Type II Different nickel window and a warmer default impact temperature. Not Type III
ASTM A353 9% nickel steel plate 9% nickel double-normalized and tempered plate; no Type split Double-normalized and tempered Yield 75 ksi [515 MPa] min; impact −320 °F [−195 °C] Orders written to A353 Different nickel level, heat treatment and yield. Not a Type III substitute
GB/T 713.4-2023 06Ni7DR Chinese 7% nickel low-temperature vessel plate Quenched and tempered or double-quenched and tempered on our 06Ni7DR page From our live 06Ni7DR page: about 7% nickel under GB/T 713.4-2023; yield 550 MPa in the mid-thickness band and 540 MPa above that; tensile 680–820 MPa; delivery quenched and tempered or double-quenched and tempered; lateral expansion not less than 0.64 mm. This is closer to A553 Type III (nominal 7% nickel) than to Type II (nominal 8% nickel). 7Ni vessel plate under GB/T 713.4-2023 Near comparison only. Closest live Chinese 7% nickel page, not an A553 Type III stamp
EN 10028-4 X8Ni9 European 9% nickel grade, steel number 1.5662 Usually quenched and tempered on our X8Ni9 page From our live X8Ni9 page: steel number 1.5662; nickel about 8.50–9.50% (the 8 in X8Ni9 is not 8% nickel); delivery usually quenched and tempered; yield in the 490 MPa class after QT; tensile 640–840 MPa; Charpy specified at −196 °C when the order follows that grade. 9Ni vessel plate Not 7% nickel and not Type III
ASME SA203 Grade E Nickel-alloy pressure-vessel plate in the normalized SA203 family. Normalized. Use its own ordered specification, thickness and delivery condition; no strength or toughness value is transferred to this grade. Low-temperature process vessels and refrigerated containment. Lower-nickel comparison, not a cryogenic-temperature substitute for ASTM A553 Type III 7% Nickel Steel Plate. Its Code edition, strength, impact temperature and certification must be selected separately.

Related published ranges: EN 10028-4 and GB/T 713.4-2023.

Equivalent and related grades by country

Near comparisons only. Type III is the official 7% nickel type in ASTM A553/A553M. Do not invent extra A553 grades beyond Type I, Type II and Type III.

Country / region Standard Grade or designation Similarity and key differences Substitution caveat
United States ASTM A553/A553M-22 Type III (nominal 7% nickel) This plate. Quenched and tempered 7% nickel. Numerical chemistry and tensile tables on this page are from ASTM A553/A553M-17 as published in ASME BPVC.II.A-2023 SA-553/SA-553M. The current ASTM publication is A553/A553M-22; name the edition on the order. This product
United States ASME SA-553/SA-553M Type III BPVC.II.A-2023 marks SA-553/SA-553M identical with ASTM A553/A553M-17, which already includes Type III, not with A553/A553M-22. Not an automatic dual stamp.
United States ASTM A553 Type I and Type II 9% and 8% nickel types Official sister types in the same specification, not optional extras. Different Types.
China GB/T 713.4-2023 06Ni7DR From our live 06Ni7DR page: about 7% nickel under GB/T 713.4-2023; yield 550 MPa in the mid-thickness band and 540 MPa above that; tensile 680–820 MPa; delivery quenched and tempered or double-quenched and tempered; lateral expansion not less than 0.64 mm. This is closer to A553 Type III (nominal 7% nickel) than to Type II (nominal 8% nickel). Near comparison only. Not an ASTM Type III designation.
Europe EN 10028-4 No live 7% nickel grade on this site X8Ni9, X7Ni9 and X10Ni9 are 9% nickel grades. 12Ni14 is about 3.25–3.75% nickel. Do not force an EN 9Ni or 3.5Ni name onto Type III.
Japan JIS G3127 No verified 7% nickel official grade stated here Live-site citations to JIS G3127 refer to 9% nickel plate such as SL9N590. Do not invent a JIS Type III equivalent.

Why choose SHH STEEL for ASTM A553 Type III

  • We produce and export ASTM A553 Type III 7% nickel steel plate
  • We review the enquiry for the named standard edition, type or designation, heat treatment, dimensions and any extra tests
  • We keep ASTM and ASME orders distinct unless the purchase order requires dual documentation and both texts can be met
  • We keep A353 double-normalizing distinct from A553 quenching and tempering, and Type I distinct from Type II
  • We match the inspection document to what the purchase order requires

How to enquire for ASTM A553 Type III plate

Item What to specify
Standard and type ASTM A553 Type III (name the Type) and the ASTM edition required; the current ASTM publication is A553/A553M-22
Heat treatment Water quenched and tempered; Type III tempering range; say if QTT is required
Dimensions Required thickness, width and length
Chemistry Heat and product analysis for Type III, including molybdenum and niobium; name the ASTM edition required on the order
Mechanical tests Tension to Table 2 of the ordered edition; Charpy V-notch at −320 °F [−195 °C] unless otherwise agreed
Other tests S55/S56 or NDE only when written on the order
Documentation State the inspection document type required by the project
Code documents If ASME SA-553 Type III documents are also required, say so explicitly and name the Section II edition

Thickness, width and length are taken from the enquiry. This page does not list stock sizes, mill capacity or fabrication services.

Request a quotation

Contact SHH STEEL for a quotation for ASTM A553 Type III 7% nickel steel plate. Please include your required quantity, plate thickness, width and length, delivery destination and preferred delivery schedule so we can review your production and export requirements.

Specify ASTM A553 Type III, the ASTM edition required (the current publication is A553/A553M-22), and water-quenched and tempered delivery. Type III is not Type I or Type II and is not 06Ni7DR unless you also want that Chinese grade reviewed separately. Include QTT, impact, NDE or SA-553 Type III documents if the project requires them.

If you are considering a related European, Chinese or Japanese nickel steel grade as an alternative, send the applicable standard and project specification with your enquiry. We will review the differences in chemistry, heat treatment, impact rules and documentation rather than assume that related grades are interchangeable.

For a detailed quotation, email your material specification, quantity and delivery requirements to our team.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X