ASTM A265 SA516 Gr.60 + Monel 400 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.60 + Monel 400 clad plate bonds nickel-copper alloy 400 (UNS N04400) to a lower-carbon SA516 Grade 60 pressure vessel base. It suits HF alkylation, crude overhead and seawater vessels at moderate pressure, with good weld hardness control. SHH STEEL produces it by explosion bonding with shear and UT tests.
Keywords
SA516 Gr.60 + Monel 400 clad plate, Monel 400 clad steel plate, ASTM A265 Monel Grade 60, N04400 clad plate, HF alkylation clad plate
Equivalent Grades:
ASME SA-265, JIS G3602, NB/T 47002.2; Monel 400 = N04400 / 2.4360 / NCu30; SA516 Gr.60 ≈ Q245R / P265GH (approx.)
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A265 SA516 Gr.60 + Monel 400 nickel alloy clad plate?

ASTM A265 SA516 Gr.60 + Monel 400 nickel alloy clad plate is a composite plate in which alloy 400 (UNS N04400, widely known as Monel 400), a nickel-copper alloy, is metallurgically bonded to an SA516 Grade 60 carbon steel base. Grade 60 is the lower-strength, lower-carbon member of the A516 family; the Monel face resists hydrofluoric acid, seawater and reducing chlorides. It is ordered to ASTM A265 or ASME SA-265.

It is written SA516 Gr.60 + N04400 or SA516 Gr.60 + Monel 400 with the thickness pair, for example 3 + 16 mm. The Grade 60 base is chosen for moderate design pressures, for heads that are heavily cold formed, and where the owner prefers a softer, tougher base with lower carbon for welding.

Monel clad plate on Grade 60 is common in HF alkylation equipment and in crude column overhead sections operating at modest pressure, where the extra strength of Grade 70 is not needed and the lower carbon helps meet hardness limits in the weld zone.

SHH STEEL can produce Monel 400 clad plate on SA516 Gr.60 by explosion bonding and certifies each plate to the A265 tests on the order. Other claddings are listed under nickel alloy clad plates.

ASTM A265 / ASME SA-265 requirements for Monel 400 clad plate

ASTM A265 covers plate of a carbon or low-alloy steel base with nickel or a nickel-base alloy integrally and continuously bonded to one or both faces. It is written mainly for pressure vessels but may be used in other structural applications where corrosion resistance is needed. ASME publishes it as SA-265, identical with ASTM A265-12(2019).

Item Requirement for SA516 Gr.60 + Monel 400
Cladding B127 / SB-127 UNS N04400 (alloy 400)
Other permitted claddings Alloys of B127, B162, B168, B333, B409, B424, B443, B463, B575, B582, B625, or others agreed
Base steel SA516 Grade 60; the standard allows pressure vessel or general structural steels (A20/A20M or A6/A6M)
Product size “Plate” means 3/16 in (4.8 mm) and over in thickness and over 10 in (254 mm) wide
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser requires them
Bond integrity Visual below 10 mm total; ultrasonic to A578/A578M procedures at 10 mm and over; Class 1, 3 or 5
Clad surface As-rolled, blasted (descaled and pickled) or 100 % conditioned, unless otherwise specified
Marking Per A20 or A6 for the base, plus the alloy designation and the specification number

A complete order line reads: “Clad plate to ASME SA-265, cladding SB-127 UNS N04400, annealed, 3 mm minimum; base SA-516 Grade 60, 16 mm minimum, normalized; Class 1 bond quality, 100 % UT (S12); shear test required; simulated PWHT per S3.” For HF service, add the hardness limits and any other requirements from the licensor’s specification.

SA516 Gr.60 base and Monel 400 cladding

A265 certifies each layer to its own specification: the cladding to ASTM B127 and the base to ASTM A516 / ASME SA-516. The pairing puts an expensive corrosion alloy only on the wetted face.

Why Monel 400 is chosen

Alloy 400 contains at least 63.0 % nickel and 28.0 to 34.0 % copper, with iron limited to 2.5 % and manganese to 2.0 %. Without chromium it does not rely on a passive film; instead its high nickel and copper make it inherently resistant in reducing media. It is one of the few engineering alloys widely used in hydrofluoric acid, and it resists seawater and chloride stress corrosion cracking.

Its weak points follow from the same chemistry. Oxidizing acids such as nitric acid, and oxidizing salts such as ferric or cupric chlorides, attack it rapidly. In moist, aerated HF vapour it can suffer stress corrosion cracking, which is why HF licensors control hardness and residual stress.

SA516 Grade 60 base steel

ASME SA516 Grade 60 is the lower-strength member of the A516 family: 415 to 550 MPa tensile strength and 220 MPa minimum yield, with lower carbon than Grade 70 and correspondingly easier welding and forming. It is supplied as-rolled or normalized and can be impact tested for low design temperatures.

Grade 60 is chosen as a clad plate base when the design pressure is modest, when heavy cold forming of heads is planned, or when the owner’s specification prefers a lower-carbon, tougher base. If a thinner shell is wanted, SA516 Grade 70 gives about 18 % more allowable stress.

SA516 Grade 60 or Grade 70 under Monel 400?

Point SA516 Gr.60 SA516 Gr.70
Tensile strength 415 – 550 MPa 485 – 620 MPa
Yield strength, min 220 MPa 260 MPa
Carbon max, 12.5 to 50 mm 0.23 % 0.28 %
Weld zone hardness Lower, easier to meet HF service limits Higher; may need controls
Typical choice Moderate pressure, formed heads, HF units Higher pressure, thinner walls

Both grades are normally supplied normalized for clad plate in HF service, because the owner specifications usually ask for fine-grained, impact-tested steel with hardness control at welds.

Alloy 400 compared with other nickel alloy claddings

Cladding Key alloying, % Typical reason to choose it
Alloy 400 (N04400) Ni 63 min, Cu 28–34 Hydrofluoric acid, seawater, crude overheads
Alloy 825 (N08825) Ni 38–46, Cr 19.5–23.5, Mo 2.5–3.5 Sulfuric and phosphoric acid, sour service
Alloy 625 (N06625) Cr 20–23, Mo 8–10 Chloride pitting, oxidizing media
Alloy C276 (N10276) Mo 15–17, Cr 14.5–16.5 Strong reducing acids, wet chlorine

How Monel 400 clad plate is made

Explosion bonding is the main manufacturing route for nickel alloy clad plate, because it joins alloys of very different strength and melting behaviour without melting either one. Roll bonding is also possible for some nickel alloys and plate sizes, and weld overlay is the alternative for shapes that cannot be clad as plate.

Explosion bonding

The Monel 400 sheet is positioned above the SA516 Gr.60 plate with a controlled gap and covered with explosive. The detonation accelerates the cladding onto the base at an oblique angle; surface oxides are jetted away and the metals bond in the solid state with a wavy interface. There is no dilution, so the cladding chemistry at the surface is exactly that of the sheet. A265 permits the cladding to be made from several sheets welded together for plates wider than the available alloy sheet, with that welding qualified to ASME Section IX.

Clad plate or weld overlay?

Monel overlay with ERNiCu-7 is used on nozzles and flanges, but iron from the steel dilutes the first layers and two or more layers are needed for a reliable surface. A Monel 400 clad plate has no dilution: its 3 mm cladding is 3 mm of B127 alloy, inspected by ultrasonic testing before fabrication.

Chemical composition of Monel 400 cladding and SA516 Gr.60 base

The chemical composition is certified layer by layer by the clad plate manufacturer: the cladding to ASTM B127 and the base to SA-516.

Monel 400 cladding (UNS N04400), heat analysis

Element Monel 400 (UNS N04400), % (ASTM B127)
Nickel (Ni), by difference 63.0 min
Copper (Cu) 28.0 – 34.0
Iron (Fe) 2.5 max
Manganese (Mn) 2.0 max
Carbon (C) 0.3 max
Silicon (Si) 0.5 max
Sulfur (S) 0.024 max

These are the B127 limits for UNS N04400; nickel is determined by difference. Product analysis of the alloy plate, when required, is made to ASTM B906 tolerances.

Product analysis of the cladding is made only when the purchaser asks for it, and the results must meet the cladding specification. For wet chemical analysis A265 asks the laboratory to discard all base metal plus 40 % of the cladding thickness from the bonded side, up to 1.6 mm, so that iron from the steel does not distort the result; spectrometric samples are taken on the centre line of the cladding.

SA516 Grade 60 base steel

Element SA516 Gr.60 heat analysis, % SA516 Gr.60 product analysis, %
Carbon (C), 12.5 mm and under 0.21 max 0.21 max
Carbon (C), over 12.5 to 50 mm 0.23 max 0.23 max
Carbon (C), over 50 to 100 mm 0.25 max 0.25 max
Carbon (C), over 100 mm 0.27 max 0.27 max
Manganese (Mn), 12.5 mm and under 0.60 – 0.90 0.55 – 0.98
Manganese (Mn), over 12.5 mm 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Grade 60 plates 12.5 mm and under may also have 0.85 to 1.20 % manganese by heat analysis. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength

A265 tests the tensile properties, the bond strength and the bond integrity of the plate in its delivered condition.

Tensile test

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base minimum up to base maximum plus 35 MPa
Composite over 38 mm, or stronger base Base steel only All base steel tensile requirements
Cladding for corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property Monel 400 cladding (ASTM B127) SA516 Gr.60 base
Tensile strength 485 MPa min (hot-rolled, annealed) 415 – 550 MPa
Yield strength (0.2 % offset) 195 MPa min 220 MPa min
Elongation 35 % min 25 % min in 50 mm; 21 % min in 200 mm
Hardness Not specified in B127 Not specified

B127 also lists hot-rolled, as-rolled plate at higher strength; clad plate is normally made with annealed sheet. SA516 Gr.60 has a minimum tensile strength below 485 MPa and a minimum yield below 275 MPa, so a composite of 38 mm or less is tested full thickness, with acceptance from 415 to 585 MPa. Alloy 400 is a little stronger than Grade 60, so the composite tends to sit in the upper half of that band.

Shear and bend tests

When required, the minimum shear strength between cladding and base is 20 000 psi (140 MPa), with at least 1.9 mm of cladding on the specimen and one test per plate as rolled. As an alternative, three bond bend tests through 180° with the cladding in compression are made; at least two must show no more than 50 % separation on either edge.

Ultrasonic bond quality

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

The class must be listed on the order; when none is given, plates may be supplied as Class 5. Scanning extent is the manufacturer’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. HF alkylation vessels and crude column tops are normally ordered Class 1 with 100 % coverage.

Heat treatment of Monel 400 clad plate

A265 does not impose a single heat treatment. Unless the cladding or base specification requires a specific treatment, or the purchaser and manufacturer agree otherwise, the clad plate is furnished in a condition appropriate for the cladding alloy, the base metal, or both.

Monel 400 clad plate is usually supplied as-clad and flattened, or stress relieved by agreement, with the alloy sheet annealed before bonding. Alloy 400 tolerates the base steel’s stress relief and PWHT without metallurgical damage.

For HF service, stress relief of the finished vessel is often required to reduce the risk of stress corrosion cracking. Like other nickel alloys, Monel must be kept clean of sulfur-bearing contaminants such as marking crayons, oils and some fuels before any heat treatment, because sulfur embrittles nickel alloys at high temperature.

If the vessel will be post-weld heat treated, order Supplementary Requirement S3 so the test coupons see a simulated PWHT, and state temperature, holding time and number of cycles.

For SA516 Gr.60 + Monel 400, normalizing of the base, when required, is done before bonding wherever possible; alloy 400 tolerates a normalizing cycle, but the base and the bond are easier to control when the clad plate is only flattened and stress relieved afterwards.

Thickness tolerances and surface finish

Cladding, base and total thickness may each be ordered as minimum or nominal values.

Item ASTM A265 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness A20/A20M or A6/A6M, as appropriate for the base

Order the alloy 400 cladding to a minimum thickness, usually 2 to 3 mm for shells and more for tube sheets. The clad surface is supplied as-rolled, blasted or conditioned.

Stock sizes and thickness combinations of Monel 400 clad plate

SA516 Gr.60 + Monel 400 clad plate is ordered by cladding plus base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 10 12 Seawater ducts
3 + 12 15 Brine vessels
3 + 14 17 HF settlers, low pressure
3 + 16 19 Column shells
3 + 20 23 Crude column top sections
4 + 25 29 Formed heads
5 + 40 45 Tube sheets
6 + 50 56 Large tube sheets
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

For nickel alloys, the cladding is usually 2 to 6 mm because of alloy cost; tube sheets take thicker layers so that tube-to-tubesheet welds stay inside the alloy.

Welding SA516 Gr.60 + Monel 400 clad plate

Clad joints are welded in two parts: a carbon steel weld for strength, then a nickel alloy overlay that restores the Monel 400 face. Carbon steel filler must not reach the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back from the root.
  2. Weld the SA516 Gr.60 with matching carbon steel filler (E7018 / ER70S-6 type), which comfortably overmatches the Grade 60 strength.
  3. Back-gouge the clad side to sound weld metal.
  4. Overlay the carbon steel weld with ERNiCu-7 (AWS A5.14) or ENiCu-7 (AWS A5.11), which match alloy 400, using enough layers to bring iron dilution at the surface within the limit the service needs.
  5. Clean the finished overlay; nickel alloys are not normally pickled like stainless steel, but heat tint and slag must be removed.

ERNiCu-7 can absorb only a limited amount of iron dilution, so many procedures first butter the steel weld with a nickel filler such as ERNi-1 and then cap with ERNiCu-7. Keep the joint free of sulfur, lead and other low-melting contaminants, which cause hot cracking in nickel-copper weld metal.

Procedures and welders are qualified to ASME Section IX, which A265 also requires for welded cladding and for cladding repairs. Repairs are checked by liquid penetrant and reported on the certificate.

Grade 60’s lower carbon makes the steel side easy to weld without preheat at normal thicknesses. On the clad side, ENiCu-7 / ERNiCu-7 is applied over an ERNi-1 buffer, which tolerates iron dilution from the steel better than nickel-copper filler alone.

Applications of Monel 400 clad plate

Monel 400 clad plate is used where nickel-copper corrosion resistance is needed in a thick or large pressure vessel.

  • HF alkylation units: acid settlers, isostrippers and HF regenerators.
  • Crude distillation columns: top sections and overhead equipment exposed to condensing HCl.
  • Seawater and brine equipment: desalination vessels and brine heaters.
  • Chlorinated solvent and organic chloride processing.
  • Hydrofluoric acid and fluorine chemicals production.
  • Caustic and salt evaporators where nickel-copper resistance is preferred.

Monel 400 clad plate vs solid alloy 400

Solid alloy 400 suits small parts and thin shells. For vessel walls over about 10 mm and for tube sheets, a Monel clad plate saves most of the alloy, and the steel base welds to carbon steel shells with standard procedures.

Why SA516 Gr.60 as the base

Grade 60 is chosen when the design pressure is moderate and the vessel benefits from a lower-carbon base: hardness in welds and HAZ is easier to keep within the limits HF alkylation specifications set, and cold-formed heads have more ductility in reserve.

Grade 60 also tolerates the extra cold work of dished and flanged heads better, which reduces the risk of cracking at knuckles during forming of thick clad heads.

Testing and certification

The A265 certificate reports the chemical analysis of both layers, the Section 7 test results, the bond quality class and any additional tests on the order.

Test or document Basis Frequency / note
Chemical analysis of both layers SA-516 and ASTM B127 Each heat; product analysis (S2) if ordered
Tensile test A265 and the base specification Each plate as rolled
Shear test or three bond bend tests A265 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Hardness survey of cladding and welds Licensor specification HF service; when ordered
Penetrant test of cladding repairs A265 Section 14 Each repair, reported with location and procedure
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

If your project does not accept weld repairs of the cladding, or wants to approve them first, state that restriction on the order; A265 lists it as a purchaser option.

Equivalent standards and grades

Other standards describe the same product with their own test levels; use them to cross-check, not to substitute without review.

Standard Scope Bond shear requirement
ASTM A265 / ASME SA-265 Nickel and nickel-base alloy-clad steel plate 140 MPa min, when specified
JIS G3602 Nickel and nickel alloy clad steels Per JIS G3602
NB/T 47002.2 Clad plate for pressure equipment, nickel-steel Per NB/T 47002.2
Layer ASTM / ASME UNS EN / W.Nr. JIS GB
Cladding B127 / SB-127 UNS N04400 (alloy 400) UNS N04400 2.4360 (NiCu30Fe) NW4400 NCu30
Base A516 / SA-516 Grade 60 K02100 P265GH (approx.) SGV410 (approx.) GB/T 713 Q245R (approx.)

Chinese projects order the same product under NB/T 47002.2 with NCu30 cladding on Q245R; Japanese projects use JIS G3602. Treat these as close equivalents and verify against the design code.

Why order Monel 400 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying nickel alloy clad plate to vessel, heat exchanger and FGD fabricators. For Monel 400 orders, often for HF or crude units, we confirm licensor requirements such as hardness and PWHT before quoting. For SA516 Gr.60 orders we confirm normalizing and impact test requirements of the base with you before bonding.

  • We check the enquiry against ASTM A265 and flag missing items: cladding specification, bond class, shear test, PWHT simulation.
  • We quote cladding and base thicknesses separately, as minimum or nominal.
  • The nickel alloy sheet and the base plate come with traceable mill certificates; UT maps are supplied when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut to drawing.

FAQ

Where is Monel 400 clad plate used?
Mainly in HF alkylation units, crude distillation column tops, seawater and brine equipment, and chlorinated organic processing, where alloy 400's nickel-copper chemistry resists corrosion.
What are the limits of Monel 400 cladding?
It is attacked by oxidizing acids such as nitric acid and by oxidizing salts like ferric chloride, and it can crack in moist aerated HF vapour if hardness and stress are not controlled.
Which filler metals weld SA516 Gr.60 + Monel 400?
Carbon steel filler such as E7018 for the base, then an ERNi-1 buffer and ERNiCu-7 / ENiCu-7 caps on the clad side.
What is the chemistry of Monel 400 cladding?
B127 requires nickel 63.0 % minimum, copper 28.0 to 34.0 %, iron 2.5 % maximum, manganese 2.0 %, carbon 0.3 %, silicon 0.5 % and sulfur 0.024 % maximum.
Is ASME SA-265 the same as ASTM A265?
Yes in content. ASME publishes A265 as SA-265 in Section II Part A, identical with ASTM A265-12(2019). Order SA-265 for ASME Code vessels.
What is the HS code for nickel alloy clad plate?
Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
ASTM A265 or ASME SA-265, Monel 400 cladding thickness and specification, base grade and thickness, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, and certificate type.

Request a quotation for ASTM A265 SA516 Gr.60 + Monel 400 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.60 + Monel 400 nickel alloy clad plate bonds B127 alloy 400 to an SA516 Grade 60 base, with 140 MPa shear strength when specified and ultrasonic Class 1, 3 or 5. It is the economical way to use nickel-copper alloy in HF alkylation, crude unit and seawater vessels.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other claddings on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *


      X