ASTM A265 SA516 Gr.70 + Inconel 625 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.70 + Inconel 625 clad plate bonds alloy 625 (UNS N06625) to a carbon steel pressure vessel base by explosion bonding. It resists pitting, crevice corrosion and chloride stress corrosion in seawater, FGD and chemical service. SHH STEEL produces it in common thickness pairs, tested for 140 MPa bond shear and ultrasonic integrity when ordered.
Keywords
Inconel 625 clad plate, alloy 625 clad steel plate, ASTM A265 625, SA516 Gr.70 + N06625, nickel alloy clad plate
Equivalent Grades:
ASME SA-265, JIS G3602, NB/T 47002.2; 625 = N06625 / 2.4856 / NS3306
Share:
General Description
Material Specification
Base and Cladding Materials
Bonding Methods
Chemical Composition
Mechanical Properties
Heat Treatment
Tolerances
Available Sizes
Weldability
Applications
Testing and Certification
Equivalent Material Grade
Why choose Us
FAQ
Conclusion

What is ASTM A265 SA516 Gr.70 + Inconel 625 nickel alloy clad plate?

ASTM A265 SA516 Gr.70 + Inconel 625 nickel alloy clad plate is a composite plate in which alloy 625 (UNS N06625, widely known as Inconel 625), a nickel-chromium-molybdenum-niobium alloy, is metallurgically bonded to an SA516 Grade 70 carbon steel base. The carbon steel carries pressure and structural loads; the nickel alloy face resists the corrosive medium. It is ordered to ASTM A265, or the identical ASME SA-265, the specification for nickel and nickel-base alloy-clad steel plate.

Fabricators write it as SA516 Gr.70 + N06625, SA516 Gr.70 + Inconel 625 or SA516 Gr.70 + alloy 625, with the thickness pair such as 3 + 20 mm. Alloy 625 is one of the most versatile corrosion alloys: about 21 % chromium and 9 % molybdenum give it very high resistance to pitting and crevice attack, and its niobium addition strengthens the matrix. Solid 625 plate is costly, so an Inconel 625 clad plate is often the only economical way to use it in thick pressure equipment.

Most buyers know 625 from weld overlay on valves and pipe. As a clad plate it does the same job over large flat areas: vessel shells, heads and tube sheets, with a uniform, undiluted alloy layer.

SHH STEEL can produce Inconel 625 clad plate by explosion bonding, the usual route for nickel alloy claddings, and certifies each plate to the A265 tests on the order. Other nickel alloy claddings are listed under nickel alloy clad plates.

ASTM A265 / ASME SA-265 requirements for Inconel 625 clad plate

ASTM A265 covers plate of a carbon or low-alloy steel base with nickel or a nickel-base alloy integrally and continuously bonded to one or both faces. It is written mainly for pressure vessels but may be used in other structural applications where corrosion resistance is needed. ASME publishes it as SA-265, identical with ASTM A265-12(2019).

Item Requirement for SA516 Gr.70 + Inconel 625
Cladding B443 / SB-443 UNS N06625 (alloy 625)
Other permitted claddings Alloys of B127, B162, B168, B333, B409, B424, B443, B463, B575, B582, B625, or others agreed
Base steel SA516 Grade 70; the standard allows pressure vessel or general structural steels (A20/A20M or A6/A6M)
Product size “Plate” means 3/16 in (4.8 mm) and over in thickness and over 10 in (254 mm) wide
Bond strength 140 MPa (20 000 psi) minimum shear, or three bond bend tests, when the purchaser requires them
Bond integrity Visual below 10 mm total; ultrasonic to A578/A578M procedures at 10 mm and over; Class 1, 3 or 5
Clad surface As-rolled, blasted (descaled and pickled) or 100 % conditioned, unless otherwise specified
Marking Per A20 or A6 for the base, plus the alloy designation and the specification number

A complete order line reads: “Clad plate to ASME SA-265, cladding SB-443 UNS N06625 Grade 1, 3 mm minimum; base SA-516 Grade 70, 20 mm minimum; Class 1 bond quality, 100 % UT (S12); shear test required; simulated PWHT per S3.” Naming the B443 grade matters, because B443 distinguishes Grade 1 (annealed) from Grade 2 (solution annealed) material.

SA516 Gr.70 base and Inconel 625 cladding

A265 certifies each layer to its own specification: the cladding to ASTM B443 and the base to ASTM A516 / ASME SA-516. The pairing puts an expensive corrosion alloy only on the wetted face.

Why Inconel 625 is chosen

Alloy 625 contains 20.0 to 23.0 % chromium, 8.0 to 10.0 % molybdenum, 3.15 to 4.15 % niobium plus tantalum and at least 58 % nickel, with iron limited to 5.0 %. The combination of chromium and molybdenum gives resistance to both oxidizing and reducing media and an extremely high resistance to chloride pitting; the high nickel makes it practically immune to chloride stress corrosion cracking.

625 is also strong. Its minimum yield in annealed plate, 379 MPa, is well above that of the stainless steels, which helps the clad face resist erosion in slurries and high-velocity flow. Its weakness, if any, is price; where the medium allows, alloy 825 or a super-austenitic stainless steel costs less.

SA516 Grade 70 base steel

ASME SA516 Grade 70 is the usual base: a carbon-manganese vessel plate with 485 to 620 MPa tensile and 260 MPa minimum yield, available normalized and impact tested. Outside ASME work it is bought as ASTM A516 Grade 70. For high-temperature hydrogen or creep service, a Cr-Mo base such as ASTM A387 Grade 11 Class 2 can replace it.

Alloy 625 compared with other nickel alloy claddings

Cladding Key alloying, % Typical reason to choose it
Alloy 625 (N06625) Cr 20–23, Mo 8–10, Nb+Ta 3.15–4.15 Seawater, chloride pitting, FGD, mixed acids
Alloy 825 (N08825) Ni 38–46, Cr 19.5–23.5, Mo 2.5–3.5, Cu 1.5–3 Sulfuric and phosphoric acid
Alloy C276 (N10276) Mo 15–17, Cr 14.5–16.5, W 3–4.5 Strong reducing acids, wet chlorine
Alloy 400 (N04400) Ni-Cu Hydrofluoric acid, seawater

How Inconel 625 clad plate is made

Explosion bonding is the main manufacturing route for nickel alloy clad plate, because it joins alloys of very different strength and melting behaviour without melting either one. Roll bonding is also possible for some nickel alloys and plate sizes, and weld overlay is the alternative for shapes that cannot be clad as plate.

Explosion bonding

The Inconel 625 sheet is positioned above the SA516 plate with a controlled gap and covered with explosive. The detonation accelerates the cladding onto the base at an oblique angle; surface oxides are jetted away and the metals bond in the solid state with a wavy interface. There is no dilution, so the cladding chemistry at the surface is exactly that of the sheet. A265 permits the cladding to be made from several sheets welded together for plates wider than the available alloy sheet, with that welding qualified to ASME Section IX.

Clad plate or weld overlay?

Weld overlay with 625 filler is common on nozzles and complex parts, but each layer picks up iron from the steel, and two or more layers are often needed to reach a low surface iron content. An explosion bonded 625 clad plate has no dilution at all, so a 3 mm cladding is 3 mm of full-chemistry alloy 625, inspected by UT before fabrication.

Chemical composition of Inconel 625 cladding and SA516 Gr.70 base

The chemical composition is certified layer by layer by the clad plate manufacturer: the cladding to ASTM B443 and the base to SA-516.

Inconel 625 cladding (UNS N06625), heat analysis

Element Inconel 625 (UNS N06625), % (ASTM B443)
Nickel (Ni) 58.0 min
Chromium (Cr) 20.0 – 23.0
Molybdenum (Mo) 8.0 – 10.0
Niobium + tantalum (Nb + Ta) 3.15 – 4.15
Iron (Fe) 5.0 max
Carbon (C) 0.10 max
Manganese (Mn) 0.50 max
Silicon (Si) 0.50 max
Phosphorus (P) 0.015 max
Sulfur (S) 0.015 max
Aluminium (Al) 0.40 max
Titanium (Ti) 0.40 max
Cobalt (Co), if determined 1.0 max

The limits are those of ASTM B443 for UNS N06625. The iron limit of 5.0 % is the figure most often discussed with clad plate, because it is the reference used when judging iron pick-up in weld overlays at clad seams.

Product analysis of the cladding is made only when the purchaser asks for it, and the results must meet the cladding specification. For wet chemical analysis A265 asks the laboratory to discard all base metal plus 40 % of the cladding thickness from the bonded side, up to 1.6 mm, so that iron from the steel does not distort the result; spectrometric samples are taken on the centre line of the cladding.

SA516 Grade 70 base steel

Element SA516 Gr.70 heat analysis, % SA516 Gr.70 product analysis, %
Carbon (C), 12.5 mm and under 0.27 max 0.27 max
Carbon (C), over 12.5 to 50 mm 0.28 max 0.28 max
Carbon (C), over 50 to 100 mm 0.30 max 0.30 max
Carbon (C), over 100 mm 0.31 max 0.31 max
Manganese (Mn) 0.85 – 1.20 0.79 – 1.30
Phosphorus (P) 0.025 max 0.025 max
Sulfur (S) 0.025 max 0.025 max
Silicon (Si) 0.15 – 0.40 0.13 – 0.45
Iron (Fe) Balance Balance

Carbon, phosphorus and sulfur limits apply to heat and product analysis alike. For each 0.01 % carbon below the maximum, the manganese maximum may rise by 0.06 %, up to 1.50 % by heat analysis and 1.60 % by product analysis.

Mechanical properties and bond strength

A265 tests the tensile properties, the bond strength and the bond integrity of the plate in its delivered condition.

Tensile test

Condition Tensile test Acceptance
Composite 38 mm and under, base minimum tensile 485 MPa or less and minimum yield 275 MPa or less Full-thickness composite specimen Base minimum up to base maximum plus 35 MPa
Composite over 38 mm, or stronger base Base steel only All base steel tensile requirements
Cladding for corrosion allowance only Cladding need not be included All base steel tensile requirements

Properties of the two layers

Property Inconel 625 cladding (ASTM B443) SA516 Gr.70 base
Tensile strength 758 MPa min (Grade 1, annealed, hot-rolled plate) 485 – 620 MPa
Yield strength (0.2 % offset) 379 MPa min 260 MPa min
Elongation 30 % min 21 % min in 50 mm; 17 % min in 200 mm
Hardness Not specified in B443 Not specified

B443 Grade 2, solution annealed, has lower minimums: 690 MPa tensile, 276 MPa yield and 30 % elongation. A 3 + 20 mm plate is tested full thickness, with the composite between 485 and 655 MPa. Because 625 is much stronger than SA516 Gr.70, a thick 625 layer raises the composite; if the cladding is ordered as corrosion allowance only, A265 lets the tensile test leave it out.

Shear and bend tests

When required, the minimum shear strength between cladding and base is 20 000 psi (140 MPa), with at least 1.9 mm of cladding on the specimen and one test per plate as rolled. As an alternative, three bond bend tests through 180° with the cladding in compression are made; at least two must show no more than 50 % separation on either edge.

Ultrasonic bond quality

Class Largest single unbonded area Total unbonded area
Class 1 25 mm (1 in) longest dimension 1 % of clad surface
Class 3 75 mm (3 in) longest dimension 3 % of clad surface
Class 5 58 cm² (9 in²) 5 % of clad surface

The class must be listed on the order; when none is given, plates may be supplied as Class 5. Scanning extent is the manufacturer’s choice unless 100 % coverage, Supplementary Requirement S12, is ordered. For tube sheets and heads with 625 cladding we recommend Class 1 with 100 % coverage.

Heat treatment of Inconel 625 clad plate

A265 does not impose a single heat treatment. Unless the cladding or base specification requires a specific treatment, or the purchaser and manufacturer agree otherwise, the clad plate is furnished in a condition appropriate for the cladding alloy, the base metal, or both.

Explosion bonded SA516 Gr.70 + 625 plate is normally delivered as-clad and flattened, or stress relieved by agreement, using 625 sheet that was annealed before bonding. A full anneal of the alloy after bonding would take the carbon steel far above its normal range, so it is rarely specified.

Holding alloy 625 for long periods at intermediate temperatures can reduce its ductility. For vessels that need PWHT of the base, qualify the cycle on S3 coupons and, where the service is critical, add a corrosion test of the cladding after simulated PWHT.

If the vessel will be post-weld heat treated, order Supplementary Requirement S3 so the test coupons see a simulated PWHT, and state temperature, holding time and number of cycles.

Thickness tolerances and surface finish

Cladding, base and total thickness may each be ordered as minimum or nominal values.

Item ASTM A265 requirement
Ordered to minimum thickness Cladding, base and total not below the ordered minimums
Nominal: base steel or total 0.3 mm under
Nominal: cladding 0.8 mm under
Over-tolerance of the total Greater of 3 mm or 10 % of the ordered total, provided each minimum is met
Width, length, flatness A20/A20M or A6/A6M, as appropriate for the base

Order the 625 cladding to a minimum thickness, commonly 2 to 3 mm; alloy cost makes extra thickness expensive. The clad surface is supplied as-rolled, blasted or conditioned; tube sheet faces can be machined.

Stock sizes and thickness combinations of Inconel 625 clad plate

SA516 Gr.70 + Inconel 625 clad plate is ordered by cladding plus base thickness, width and length. SHH STEEL keeps common sizes in stock or produces them quickly, and any other pair inside the production range can be made to order.

Cladding + base, mm Total, mm Typical use
2 + 10 12 FGD ducts and absorber shells
2 + 12 14 Scrubbers
3 + 14 17 Vessel shells
3 + 16 19 Seawater equipment
3 + 20 23 Pressure vessels, separators
3 + 25 28 Heavier shells
4 + 30 34 Heads
5 + 40 45 Tube sheets
6 + 50 56 Clad tube sheets
8 + 60 and over 68 and over Large tube sheets, explosion bonded
Dimension Production range
Cladding thickness 2 mm to 20 mm (thicker by explosion bonding on request)
Base steel thickness 6 mm to 200 mm
Total thickness 8 mm to 220 mm
Width 1000 mm to 3000 mm; wider by explosion bonding with welded cladding
Length 2000 mm to 12000 mm
Discs and blanks Round tube sheet blanks and head blanks cut to drawing
Location China

For nickel alloys, the cladding is usually 2 to 6 mm because of alloy cost; tube sheets take thicker layers so that tube-to-tubesheet welds stay inside the alloy.

Welding SA516 Gr.70 + Inconel 625 clad plate

Clad joints are welded in two parts: a carbon steel weld for strength, then a nickel alloy overlay that restores the Inconel 625 face. Carbon steel filler must not reach the cladding.

  1. Prepare the joint to the qualified procedure, usually bevelled from the steel side with the cladding cut back from the root.
  2. Weld the SA516 Gr.70 with matching carbon steel filler.
  3. Back-gouge the clad side to sound weld metal.
  4. Overlay the carbon steel weld with ERNiCrMo-3 (AWS A5.14) or ENiCrMo-3 (AWS A5.11), which matches alloy 625, using enough layers to bring iron dilution at the surface within the limit the service needs.
  5. Clean the finished overlay; nickel alloys are not normally pickled like stainless steel, but heat tint and slag must be removed.

ERNiCrMo-3 can be deposited directly on the carbon steel weld metal, so a separate buffer alloy is not needed; what matters is the number of layers and the heat input, which together set the iron content of the surface. Nickel alloy weld pools are sluggish, so joint angles are opened up compared with carbon steel, and the surface must be free of sulfur, oil and marking ink before welding.

Procedures and welders are qualified to ASME Section IX, which A265 also requires for welded cladding and for cladding repairs. Repairs are checked by liquid penetrant and reported on the certificate.

Applications of Inconel 625 clad plate

Inconel 625 clad plate is used where stainless steels pit or crack and the vessel is too thick or large to make in solid alloy.

  • Flue gas desulfurization absorbers, outlet ducts and stacks with acid chloride condensate.
  • Seawater and brine equipment: separators, coolers, desalination vessels.
  • Offshore and sour gas separators and process vessels.
  • Chemical reactors with mixed acids and chlorides.
  • Heat exchanger tube sheets facing seawater.
  • Pulp bleaching equipment with chlorine dioxide.

Inconel 625 clad plate vs solid 625

Solid 625 suits thin sheet and small parts. For shells over about 10 mm, and for tube sheets, a 625 clad steel plate reduces the alloy content by 70 to 90 %, and the carbon steel side welds to standard nozzles and supports.

Testing and certification

The A265 certificate reports the chemical analysis of both layers, the Section 7 test results, the bond quality class and any additional tests on the order.

Test or document Basis Frequency / note
Chemical analysis of both layers SA-516 and ASTM B443 Each heat; product analysis (S2) if ordered
Tensile test A265 and the base specification Each plate as rolled
Shear test or three bond bend tests A265 When specified
Ultrasonic bond inspection A578/A578M procedures, Class 1/3/5 10 mm and thicker; 100 % with S12
Charpy V-notch impact Supplementary Requirement S5 When ordered for the base
Simulated PWHT of coupons Supplementary Requirement S3 When the vessel is heat treated
Corrosion test of cladding Agreed method When ordered
Penetrant test of cladding repairs A265 Section 14 Each repair, reported with location and procedure
Mill test certificate EN 10204 3.1; 3.2 with third-party inspection on request Each plate or lot

If your project does not accept weld repairs of the cladding, or wants to approve them first, state that restriction on the order; A265 lists it as a purchaser option.

Equivalent standards and grades

Other standards describe the same product with their own test levels; use them to cross-check, not to substitute without review.

Standard Scope Bond shear requirement
ASTM A265 / ASME SA-265 Nickel and nickel-base alloy-clad steel plate 140 MPa min, when specified
JIS G3602 Nickel and nickel alloy clad steels Per JIS G3602
NB/T 47002.2 Clad plate for pressure equipment, nickel-steel Per NB/T 47002.2
Layer ASTM / ASME UNS EN / W.Nr. JIS GB
Cladding B443 / SB-443 UNS N06625 (alloy 625) UNS N06625 2.4856 (NiCr22Mo9Nb) NCF625 NS3306
Base A516 / SA-516 Grade 70 K02700 P355GH (approx.) SGV480 (approx.) GB/T 713 Q345R (approx.)

Chinese projects order the same product under NB/T 47002.2 with NS3306 cladding; Japanese projects use JIS G3602. Stainless claddings for milder duty are ordered under ASTM A264/A264M.

Why order Inconel 625 clad plate from SHH STEEL

SHH STEEL is a clad plate manufacturer in China supplying nickel alloy clad plate to vessel, heat exchanger and FGD fabricators. For 625 clad plate we check the B443 grade and heat treatment of the sheet before bonding.

  • We check the enquiry against ASTM A265 and flag missing items: cladding specification, bond class, shear test, PWHT simulation.
  • We quote cladding and base thicknesses separately, as minimum or nominal.
  • The nickel alloy sheet and the base plate come with traceable mill certificates; UT maps are supplied when 100 % coverage is ordered.
  • Tube sheet discs and head blanks can be cut to drawing.

FAQ

Is Inconel 625 clad plate ordered to ASTM A264 or A265?
ASTM A265 (or ASME SA-265). A265 covers nickel and nickel-base alloy claddings, including B443 alloy 625. A264 is for stainless chromium-nickel steel claddings.
What filler metal is used for 625 clad plate?
ERNiCrMo-3 or ENiCrMo-3, matching alloy 625, applied over the carbon steel weld in enough layers to keep surface iron low. Carbon steel filler must not touch the cladding.
What is the difference between B443 Grade 1 and Grade 2?
Grade 1 is annealed, with 758 MPa tensile and 379 MPa yield minimum for hot-rolled plate. Grade 2 is solution annealed, with 690 and 276 MPa. Grade 2 is usually chosen for high-temperature creep service.
How thick should the 625 cladding be?
Usually 2 to 3 mm for shells, set by the corrosion allowance. Tube sheets often use 5 mm or more so that tube holes and seal welds stay inside the alloy.
Is ASME SA-265 the same as ASTM A265?
Yes in content. ASME publishes A265 as SA-265 in Section II Part A, identical with ASTM A265-12(2019). Order SA-265 for ASME Code vessels.
What is the HS code for nickel alloy clad plate?
Nickel alloy clad steel plate on a non-alloy steel base, 600 mm or wider, is commonly declared under HS 7210.90, flat-rolled products of iron or non-alloy steel, clad, plated or coated, other. The clad plate HS code depends on the base steel and width: narrower or alloy-steel-base plates fall under other headings, so confirm with your customs broker.
What should I send for a quotation?
ASTM A265 or ASME SA-265, Inconel 625 cladding thickness and specification, base grade and thickness, width, length or drawing, quantity, UT class and coverage, shear or bend test, heat treatment and PWHT simulation, and certificate type.

Request a quotation for ASTM A265 SA516 Gr.70 + Inconel 625 Nickel Alloy Clad Plate

ASTM A265 SA516 Gr.70 + Inconel 625 nickel alloy clad plate combines B443 alloy 625 with an SA516 Grade 70 base, explosion bonded, with 140 MPa minimum shear when specified and ultrasonic bond quality Class 1, 3 or 5. It is the clad answer for chloride pitting, seawater and FGD service.

Send the thickness pair, plate size or drawing, quantity, tests and certificate type to SHH STEEL, or compare other claddings on our nickel alloy clad plates page. Availability, testing and delivery are confirmed with each quotation.

Contact: admin@steelspecs.com

Contact Us

Quality Steel Needed? Inquire for Offers

Need quality steel for your project? Inquire now to get tailored offers. Our team ensures quick responses, matching your needs with reliable steel solutions. Start your inquiry today.

    *

    *

    *

    *


    Related Products

    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response
    SHH STEEL Get Your Steel Quote—Inquire Now for Quick Response

      *

      *

      *

      *