Equivalent grades: UNS S32760 ≈ EN 1.4501 X2CrNiMoCuWN25-7-4 ≈ GB/T 022Cr25Ni7Mo4WCuN (S27603).
UNS S32760 is a super duplex (tungsten-bearing) grade. S32760 is a 25Cr-7Ni-3.5Mo-N super-duplex grade with additions of copper and tungsten. A240 (footnote to Table 1) requires Cr + 3.3 (Mo + ½ W) + 16 N of 41 minimum for this grade; project specifications may add their own PREN formula and minimum. It is widely used for seawater and sour service.
ASTM A240/A240M covers chromium, chromium-nickel and chromium-manganese-nickel stainless steel plate, sheet and strip for pressure vessels and general applications. Under ASTM A480, sheet is flat material under 5.00 mm thick and 600 mm or more wide, so UNS S32760 sheet is a cold-rolled 2B/2D product in thin gauges and a hot-rolled, annealed and pickled No.1 product toward the 4.75 mm end.
This page sets out the ASTM A240/A240M requirements for UNS S32760 sheet: specification summary, chemistry, mechanical properties, corrosion resistance, heat treatment, finishes and tolerances, current stock, equivalents, fabrication and testing. SHH STEEL supplies it mill-direct from China with EN 10204 3.1 certificates, optional third-party inspection and in-house cutting.
UNS S32760 sheet: specification summary
| Item | UNS S32760 data |
|---|---|
| Standard | ASTM A240/A240M; general requirements ASTM A480/A480M |
| ASME counterpart | SA-240 (ordered for ASME Code construction) |
| Product form (A480) | sheet: under 5.00 mm thick, 600 mm and wider; plate 5.00 mm and over |
| Typical gauges | 0.5–3.0 mm cold-rolled 2B/2D; 3.0–4.75 mm hot-rolled No.1 |
| Widths | 1000, 1219, 1250, 1500 mm; slit coil to order |
| Lengths | 2000, 2438, 2500, 3000 mm or cut to size |
| Finishes | No.1, 2D, 2B; BA and No.4 by agreement |
| Required tests | heat analysis, tension test, hardness (and bend where the grade requires it) |
| Certificates | EN 10204 3.1; 3.2 with third-party witness on request |
| Grade family | super duplex |
Size range. Sheet is normally cold rolled from about 0.3–0.5 mm up to 3 mm and hot rolled from about 3 mm to just under 5 mm. Coil widths of 1000, 1219, 1250 and 1500 mm are standard; slitting and cut-to-length lines produce narrower strip and exact lengths. Sheets thinner than 0.5 mm or wider than 1500 mm should be confirmed before ordering. UNS S32760 is produced regularly by several mills; common sizes are held in stock, and other sizes are rolled in the mill’s scheduled campaigns for the grade.
Chemical composition of UNS S32760 (ASTM A240/A240M)
| Element | wt % |
|---|---|
| C | 0.030 max |
| Si | 1.00 max |
| Mn | 1.00 max |
| P | 0.030 max |
| S | 0.010 max |
| Cr | 24.0–26.0 |
| Ni | 6.0–8.0 |
| Mo | 3.0–4.0 |
| Cu | 0.50–1.00 |
| N | 0.20–0.30 |
| W | 0.50–1.00 |
Single values are maximums unless marked min. Ranges are heat (cast) analysis limits.
PREN check (Cr + 3.3 Mo + 16 N): about 37.1 at the specification minimums and about 40.5 at mid-range. Where corrosion resistance is critical, write a minimum PREN on the order and ask for the calculated value from the heat analysis on the certificate.
Mechanical properties of UNS S32760 sheet
| Condition / thickness | Tensile strength, min | Yield strength 0.2 %, min | Elongation in 50 mm, min | Hardness, max |
|---|---|---|---|---|
| all thicknesses | 750 MPa (109 ksi) | 550 MPa (80 ksi) | 25 % | 310 HBW / 32 HRC |
The minimum yield strength of 550 MPa is about 3.2 times the 170 MPa minimum of ASTM 316L. Designers use this to reduce thickness, but higher strength also means higher press loads and more springback. Mill values for production heats are usually well above the minimums; use certificate values when you calculate bending forces. Tension tests are taken in the direction stated in the standard; where a hardness limit is given, it is a maximum that confirms correct annealing.
Corrosion resistance of UNS S32760: PREN and limits
Super-duplex grades are duplex steels with PREN of about 40 or more. At the specification minimum this grade calculates to about 37.1, and a mid-range heat to about 40.5. That level gives resistance to pitting and crevice corrosion in ambient seawater, strong resistance to chloride stress-corrosion cracking and a yield strength above 500 MPa.
The higher alloy content makes super-duplex more sensitive to intermetallic phases than 2205. The solution-anneal temperature is higher and cooling must be fast, especially for heavy plate. Specify ASTM A923 Methods A, B and C, a ferrite range (commonly 35–55 % by ASTM E562) and, for critical service, an ASTM G48 Method A test at the temperature named in the project specification. Like all duplex grades, the upper service limit is about 250–300 °C.
How UNS S32760 compares with related grades
| Grade | Cr | Ni | Mo | N | PREN (min) | YS / Rp0.2 min, MPa |
|---|---|---|---|---|---|---|
| UNS S32760 | 24.0–26.0 | 6.0–8.0 | 3.0–4.0 | 0.20–0.30 | 37.1 | 550 |
| UNS S32906 | 28.0–30.0 | 5.8–7.5 | 1.50–2.60 | 0.30–0.40 | 37.8 | 650 |
| UNS S32550 | 24.0–27.0 | 4.5–6.5 | 2.9–3.9 | 0.10–0.25 | 35.2 | 550 |
| UNS S32520 | 24.0–26.0 | 5.5–8.0 | 3.0–4.0 | 0.20–0.35 | 37.1 | 550 |
Choose UNS S32760 for ambient seawater, chlorinated brines and high-chloride process water where 2205 is not sufficient, and where its high strength reduces weight. Do not use it above about 250–300 °C, and check that your fabricator has qualified super-duplex welding procedures.
The table uses specification limits, not typical mill values, so it shows the guaranteed position of each grade. Final selection should also consider product availability in the thickness you need, welding consumables, and the inspection requirements of your project.
Heat treatment and delivery condition of UNS S32760
Heat treatment: 1100–1140 °C, rapid cooling.
The higher alloy content gives faster intermetallic precipitation than 2205, so heavy plate must be water quenched. Hot forming is done between about 1000 and 1200 °C and must be followed by a full solution anneal and quench.
Surface finishes for UNS S32760 sheet
No.1 is hot-rolled, annealed and pickled, used for the 3–4.75 mm end of the sheet range. 2D is a dull cold-rolled, annealed and pickled finish that holds lubricant in deep drawing. 2B adds a light skin pass for a smoother, brighter surface and is the normal base for polishing. BA (bright annealed) and No.4 brushed finishes are available for many austenitic and ferritic grades by agreement. For highly alloyed grades, cold-rolled thin gauges are produced by fewer mills, so confirm the finish and gauge range before you fix a design.
Dimensions, tolerances and flatness
Thickness, width, length, flatness and camber tolerances follow ASTM A480/A480M. Cold-rolled sheet has tighter thickness tolerances than hot-rolled No.1 sheet. Higher-strength grades show more residual stress after slitting and laser cutting, so for laser blanks or long panels specify flatness and, where needed, tension-levelled material. Edge condition (mill or slit edge) and PVC film on one side should be stated on the order.
Ordering notes for A240 sheet. A240 refers to ASTM A480 for everything that is not grade-specific: definitions of sheet, strip and plate, dimensional tolerances, finishes, marking, retests and certification. A purchase order that says only “A240 S32760” therefore leaves several choices to the mill. State the finish (2B, 2D or No.1), the thickness tolerance basis, whether coil, slit coil or cut lengths are wanted, and whether the certificate must also show SA-240. If the sheet will be formed into vessel heads or pressure parts, say so, because some grades need specific heat-treatment records and supplementary tests that are only reported when requested. For export, also state the edition year if your specification fixes one; most mills certify to the current edition by default.
UNS S32760 sheet stock in China
| Thickness (mm) | Width (mm) | Length (mm) | Finish | Approx. quantity | Location |
|---|---|---|---|---|---|
| 0.5 | 1000 / 1219 | 2000 / 2438 | 2B | 200+ t | China |
| 0.8 | 1219 | 2438 | 2B | 200+ t | China |
| 1.0 | 1219 / 1250 | 2438 / 2500 | 2B | 100+ t | China |
| 1.5 | 1219 / 1500 | 2438 / 3000 | 2B | 100+ t | China |
| 2.0 | 1219 / 1500 | 2438 / 3000 | 2B | 100+ t | China |
| 3.0 | 1500 | 3000 | 2B / No.1 | 100+ t | China |
| 4.0 | 1500 | 3000 / 6000 | No.1 | 100+ t | China |
Quantities are approximate and stock changes daily. Send your size list for current availability; other thicknesses, widths and cut sizes can be supplied from mill production.
Packing and logistics. Sheet is packed on wooden or steel pallets with interleaving paper or PVC film, edge protectors and waterproof wrapping, typically 2–3 t per pallet. Coil is packed eye-to-wall or eye-to-sky with steel bands. We consolidate mixed grades and sizes into one container and send loading photos with the shipping documents.
UNS S32760 equivalents in other standards
| Standard | Designation | Comment |
|---|---|---|
| EN | 1.4501 X2CrNiMoCuWN25-7-4 | same alloy family and limits closely matched; compare each limit on the certificate |
| GB/T | 022Cr25Ni7Mo4WCuN (S27603) | same alloy family and limits closely matched; compare each limit on the certificate |
Equivalents are close, not identical. When a project names one standard, order to that standard or ask for multiple certification and check every limit on the certificate.
Related grades by alloy family
Super duplex
PREN 40+ duplex grades for seawater and severe chlorides: A240 S32750, 1.4410 plate, 1.4507 plate, A240 S32520, A240 S32550, A240 S32906.
Duplex and lean duplex
Duplex grades with about twice the yield strength of 316L: A240 S32205, A240 S32304, A240 S32101, 1.4462 plate, 1.4362 plate.
Super austenitic
6Mo and 7Mo grades for seawater and chloride service; upgrade path from 316L and 904L: A240 N08904.
Same grade, other specification
Applications, forming and welding of UNS S32760
Typical uses: offshore topsides seawater and fire-water systems, subsea manifolds, desalination, FGD equipment, and chemical-plant vessels in chloride service.
Super-duplex plate needs more press force than 2205 and careful control of cutting heat. Cut by plasma, laser or waterjet and remove heat tint by pickling or grinding. For welding use a super-duplex filler such as ER2594 (AWS A5.9) or a nickel-base filler where the specification allows it. Keep the weld area clean and free of carbon-steel contamination, and pickle and passivate after welding where corrosion resistance matters.
Welding practice. Super duplex has a narrower heat-input window than 2205, typically about 0.5–1.5 kJ/mm with interpass below 100–150 °C. Use a nitrogen-bearing shielding and backing gas, and qualify with ferrite counts in weld metal and HAZ, G48 testing and Charpy tests as the project specification requires. Avoid repair welding in the same spot more than once.
Certificates, testing and receiving inspection
Every delivery carries a mill certificate to ASTM A480/A480M with heat analysis, tensile results and hardness, and the grade and standard as ordered. Supplementary tests we can arrange: ASTM A923 Methods A, B and C, ferrite count to ASTM E562, ASTM G48 Method A at the specified temperature, Charpy impact, and PMI on each plate. Third-party witness by SGS, BV, TÜV, DNV, ABS or LR is available with EN 10204 3.2 certificates.
On receipt, check marking and heat number against the certificate, measure thickness at several points and confirm the finish and edge condition before cutting.
Common mistakes when specifying UNS S32760
- Not stating whether PREN includes tungsten.
- Accepting heavy plate without A923 results; intermetallics are invisible on the surface.
- Using a 2205 welding procedure for super duplex.
Each of these can be avoided by writing the requirement into the purchase order and checking it on the certificate before the material is cut.
Sourcing UNS S32760: buyer concerns and SHH STEEL solutions
| Concern | How SHH STEEL handles it |
|---|---|
| Sigma phase in heavy plate | A923 A/B/C and G48 results reviewed per heat before cutting |
| PREN definition (with or without W) | formula and minimum fixed in the purchase order |
| Small quantities across many sizes | mixed thicknesses and grades combined in one shipment |
| Cutting and edge preparation | in-house shearing, plasma, laser and waterjet cutting, bevelling |
| Delivery delays | weekly production and shipping updates with photos |
How to order UNS S32760 sheet
State the standard and edition (ASTM A240/A240M), the grade (UNS S32760), thickness, width and length or coil, finish, quantity, tolerance class, any added chemistry limits, the supplementary tests and acceptance values from your specification, the certificate type and inspection agency, and packing. Send the list to SHH STEEL and we will reply with price, available stock and lead time.
FAQ
-
Can I use A240 S32760 sheet for ASME Code equipment?
- Only if it is certified to SA-240 as well. Most mills dual-certify A240/SA-240; tell us when the sheet is for Code construction and we will supply dual-marked material with the certificate stating both.
-
Is UNS S32760 equivalent to EN 1.4501 X2CrNiMoCuWN25-7-4?
- They are the same alloy designation in different standards. Limits are closely matched, but always order to the standard named in your specification or ask for multiple certification.
-
Should PREN include tungsten?
- Only if your specification says so. Some specifications use Cr + 3.3 Mo + 16 N, others Cr + 3.3 (Mo + 0.5 W) + 16 N; write the formula and the minimum on the order.
-
Can I order small quantities or cut sizes?
- Yes. We combine mixed thicknesses and grades into one shipment and cut plate and sheet to size in our workshop.
-
Which certificates and tests can you provide?
- Every order ships with a mill certificate (EN 10204 3.1 type) showing heat analysis and mechanical tests. Supplementary tests and 3.2 certificates with SGS, BV, TÜV or another agency are available by agreement.
Conclusion
UNS S32760 sheet should be ordered with the points the standard leaves open written into the contract: finish, tolerance class, any extra chemistry limits and the supplementary tests your application needs. With those fixed, stock material from China is a fast and reliable route.